Hot air preparation method of polylactic acid composite non-woven fabric with high air permeability and high strength

Through the preparation technology of modified polylactic acid fiber and hot air nonwoven, the problem of difficulty in taking into account both breathability and strength of polylactic acid nonwoven is solved, and a high breathability and high strength polylactic acid composite nonwoven is achieved, which is suitable for multiple A kind of application scenario.

CN118979337AActive Publication Date: 2024-11-19SHENZHEN ESUN IND +1

Patent Information

Application Number
CN202411134429.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-19
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Existing polylactic acid nonwovens are difficult to take into account both breathability and strength. Traditional preparation processes may lead to uneven fiber distribution, affecting breathability, and excessive heat pressing treatment will reduce breathability.

Method used

Preparation steps and parameters of specific modified polylactic acid fiber and hot air nonwoven fabrics include stirring and dissolving polylactic acid in dimethylformamide and adding potassium persulfate, potassium bisulfite, etc., followed by addition of ethyl acrylate and buty acrylate. After grafting reaction, tetraethyl ammonium bromide and dilute sulfuric acid are added to form modified fibers, and melt-spinning, drafting, drying, swinging and hot air shaping through a screw extruder to form high Breathable and high-strength polylactic acid composite non-woven fabric.

Benefits of technology

It achieves a balance of high breathability and high strength of polylactic acid composite non-woven fabrics, improves the environmental performance and usage effect of the product, is suitable for medical and health care and personal care fields, and has broad market prospects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a hot air preparation method of a polylactic acid composite non-woven fabric with high air permeability and high strength, and belongs to the technical field of polylactic acid materials.The method comprises the steps that polylactic acid is stirred and dissolved in dimethylformamide, and potassium persulfate and sodium hydrogen sulfite are added; ethyl acrylate and butyl acrylate are added, and mercaptoacetic acid is added for a reaction; after trimethylolpropane triacrylate is added, triethylamine is added, and the reaction continues; separating to obtain grafted polylactic acid; dissolving the grafted polylactic acid in acetone, adding tetraethylammonium bromide for dissolving, slowly dropwise adding a dilute sulfuric acid solution, and reacting; cooling and separating to obtain modified polylactic acid; taking modified polylactic acid, polycaprolactone and an auxiliary agent, mixing, melting and spinning to form fibers, swaying, lapping and needling; carding with hot air. Modified polylactic acid fibers are prepared by adopting a specific modification reagent and method, and the high-breathability and high-strength polylactic acid composite non-woven fabric is prepared by adopting the modified polylactic acid fibers in cooperation with specific hot air non-woven fabric preparation steps and parameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polylactic acid material preparation, and specifically relates to a hot air preparation method for a high-permeability and high-strength polylactic acid composite non-woven fabric. Background Art

[0002] With the increasing awareness of environmental protection, the application of biodegradable materials in various fields has become increasingly important. Polylactic acid (PLA), a biodegradable material extracted from renewable plant resources, is an ideal choice to replace traditional plastics due to its environmental friendliness, biocompatibility and processability. In the textile field, non-woven fabrics made of polylactic acid fibers have attracted much attention due to their unique properties.

[0003] The hot air preparation method of polylactic acid composite non-woven fabric mainly uses polylactic acid fibers with a specific structure to be combed into a web, and the fiber web is reinforced by hot air shaping technology to make an environmentally friendly non-woven fabric. The advantages of this preparation method are the environmental protection in its production process, the biodegradability of the product and good physical properties. Hot air shaping can not only improve the strength of the non-woven fabric, but also maintain its good air permeability and moisture absorption, so that it performs well in various applications.

[0004] However, some PLA non-woven fabrics on the market still have some technical defects, especially in terms of air permeability and strength. The traditional non-woven fabric preparation process may cause uneven fiber distribution, which in turn affects the air permeability of the non-woven fabric. In addition, excessive heat pressing to improve strength will also reduce the air permeability of the non-woven fabric, making the final product uncomfortable for users during use.

[0005] Polylactic acid composite nonwoven fabrics are expected to solve this problem by using special fiber structures and hot air setting technology. The specific arrangement of its fibers and the temperature and pressure control during the hot air setting process are key factors affecting the air permeability and strength of nonwoven fabrics. By precisely controlling these parameters, a balance between air permeability and strength can be achieved, thereby producing nonwoven fabric products that are both environmentally friendly and high-performance.

[0006] As consumers' requirements for environmental protection and health continue to increase, the market prospects for polylactic acid composite nonwoven fabrics are broad. It is not only widely used in the fields of medical care, personal care, etc., but is also expected to become a substitute for traditional non-degradable nonwoven fabrics, contributing to the green development of the textile industry. At the same time, with further research and optimization of preparation technology, the performance of polylactic acid composite nonwoven fabrics will be further improved to meet more diverse market needs.

[0007] As an environmentally friendly and high-performance nonwoven production technology, the hot air preparation method of polylactic acid composite nonwovens has significant advantages and broad development prospects. Although there are still some technical challenges, these problems are expected to be solved through continuous research and development and innovation, promoting the wider application of polylactic acid nonwovens in various fields. Summary of the invention

[0008] In order to solve the above problems, the present invention mainly optimizes from the perspective of fiber modification and provides a hot air preparation method for high-permeability and high-strength polylactic acid composite non-woven fabric. The specific scheme is as follows:

[0009] A hot air preparation method for a high-permeability and high-strength polylactic acid composite non-woven fabric comprises the following steps:

[0010] S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well;

[0011] S2, maintaining the reaction temperature and continuing stirring, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction;

[0012] S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction;

[0013] S4, after the reaction is completed, the grafted polylactic acid is separated;

[0014] S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react;

[0015] S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid;

[0016] S7, taking the obtained modified polylactic acid, polycaprolactone, and additives and mixing them to obtain a spinning material;

[0017] S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0018] S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0019] Preferably, in S8, the melting temperature is 180-200°C, the spinning temperature is 190-230°C, the winding speed is 800-1000 m / min; the drawing temperature is 70-90°C, and the multiple is 2.2-3.5 times.

[0020] Preferably, the wire bundle spacing of the swing wire in S8 is 5-8mm, and the wire bundle tension is 1.5-2.5cN; the laying speed of the web is 20-50m / min, the laying angle is 50-80°, excluding 60°, and the number of laying layers is 5-10 layers.

[0021] Preferably, in S9, the hot air temperature is 100-130° C., the hot air speed is 4-8 m / s, and the hot air combing time is 30-50 s.

[0022] Preferably, the stirring and dissolving in S1 is carried out at 70-75°C.

[0023] Preferably, the concentration of polylactic acid in dimethylformamide in S1 is 0.3-0.5 g / mL.

[0024] Preferably, the mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is (10-15):(0.04-0.08):(0.03-0.06).

[0025] Preferably, the reaction temperature in S2 is maintained at 80-85°C.

[0026] Preferably, in S2, the ratio of ethyl acrylate to polylactic acid is 0.15-0.3 mL of ethyl acrylate per 1 g of polylactic acid; and the ratio of butyl acrylate to polylactic acid is 0.05-0.1 mL of butyl acrylate per 1 g of polylactic acid.

[0027] Preferably, the mass ratio of thioglycolic acid to polylactic acid in S2 is (0.0015-0.0025):1.

[0028] Preferably, the usage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.02-0.04 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; and the usage mass ratio of triethylamine to polylactic acid is (0.0025-0.004):1.

[0029] Preferably, the amount of acetone in S5 is 5-10 times the mass of the grafted polylactic acid.

[0030] Preferably, the mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is (0.01-0.05):1.

[0031] Preferably, the concentration of the dilute sulfuric acid solution in S5 is 0.5-1.5 mol / L; and the amount used is 15-25 vol% of the volume of acetone.

[0032] Preferably, the heating and stirring reaction in S5 is carried out at a temperature of 50-70° C. and for a time of 3-7 hours.

[0033] Preferably, the amount of polycaprolactone in S7 is 10-12 wt % of the modified polylactic acid.

[0034] Preferably, the auxiliary agent in S7 includes 2-5 wt% of phthalate in the modified polylactic acid and 0.1-0.5 wt% of calcium stearate in the modified polylactic acid.

[0035] Beneficial Effects

[0036] The invention adopts a specific modification agent and method to prepare modified polylactic acid fiber, and adopts the modified polylactic acid fiber in combination with specific hot air nonwoven fabric preparation steps and parameters to prepare a high-permeability and high-strength polylactic acid composite nonwoven fabric. DETAILED DESCRIPTION

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0039] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified. The details are as follows:

[0040] Polylactic acid particles: NatureWorks 4032D PLA, molecular weight 150,000 g / mol;

[0041] Dimethylformamide: N,N-dimethylformamide, Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No. 68-12-2;

[0042] Potassium persulfate: Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0043] Sodium bisulfite: Beekman Biotech, CAS No. 7757-83-7;

[0044] Ethyl acrylate: Nanjing Chemical Reagent Co., Ltd., 98%;

[0045] Butyl acrylate: Xilong Science, 1 mol / L;

[0046] Thioglycolic acid: ammonium thioglycolate, Jiangsu Xinsu New Materials Co., Ltd.;

[0047] Trimethylolpropane triacrylate: Shandong Xiya Chemical Co., Ltd., 85%;

[0048] Triethylamine: Hubei Weishi Chemical Reagent Co., Ltd.;

[0049] Tetraethylammonium bromide: Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0050] Polycaprolactone: Shanghai Puzhen Biotechnology Co., Ltd.;

[0051] Phthalate: dimethyl phthalate, Hubei Chengfeng Chemical Co., Ltd.;

[0052] Calcium stearate: Guangzhou Hewei Pharmaceutical Technology Co., Ltd.

[0053] Example 1 A hot air preparation method for a high-permeability and high-strength polylactic acid composite non-woven fabric:

[0054] S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well;

[0055] S2, maintaining the reaction temperature and continuing stirring, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction;

[0056] S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction;

[0057] S4, after the reaction is completed, the grafted polylactic acid is separated;

[0058] S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react;

[0059] S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid;

[0060] S7, taking the obtained modified polylactic acid, polycaprolactone, and additives and mixing them to obtain a spinning material;

[0061] S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0062] S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0063] In S8, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0064] The wire bundle spacing of S8 is 5mm, and the wire bundle tension is 1.5cN; the laying speed of the web is 20m / min, the laying angle is 50°, and the number of laying layers is 5.

[0065] In S9, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0066] The stirring and dissolving in S1 is carried out at 70°C.

[0067] The concentration of polylactic acid in S1 in dimethylformamide was 0.3 g / mL.

[0068] The mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is 10:0.08:0.06.

[0069] The reaction temperature was maintained at 80°C in S2.

[0070] In S2, the ratio of ethyl acrylate to polylactic acid is 0.15 mL of ethyl acrylate per 1 g of polylactic acid; the ratio of butyl acrylate to polylactic acid is 0.05 mL of butyl acrylate per 1 g of polylactic acid.

[0071] The mass ratio of thioglycolic acid to polylactic acid in S2 is 0.0015:1.

[0072] The usage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.02 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; the usage mass ratio of triethylamine to polylactic acid is 0.0025:1.

[0073] The amount of acetone used in S5 is 10 times the mass of grafted polylactic acid.

[0074] The mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is 0.01:1.

[0075] The concentration of the dilute sulfuric acid solution in S5 is 0.5 mol / L; the amount used is 15 vol% of the volume of acetone.

[0076] The heating and stirring reaction in S5 is carried out at a temperature of 50° C. for 3 hours.

[0077] The amount of polycaprolactone in S7 is 10 wt % of the modified polylactic acid.

[0078] The auxiliary agents in S7 include 2 wt % of phthalate modified polylactic acid and 0.2 wt % of calcium stearate modified polylactic acid.

[0079] Example 2 A hot air preparation method for a high-permeability and high-strength polylactic acid composite non-woven fabric:

[0080] S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well;

[0081] S2, maintaining the reaction temperature and continuing stirring, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction;

[0082] S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction;

[0083] S4, after the reaction is completed, the grafted polylactic acid is separated;

[0084] S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react;

[0085] S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid;

[0086] S7, taking the obtained modified polylactic acid, polycaprolactone, and additives and mixing them to obtain a spinning material;

[0087] S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0088] S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0089] In S8, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0090] The wire bundle spacing of S8 is 5mm, and the wire bundle tension is 1.5cN; the laying speed of the web is 20m / min, the laying angle is 50°, and the number of laying layers is 5.

[0091] In S9, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0092] The stirring and dissolving in S1 is carried out at 75°C.

[0093] The concentration of polylactic acid in dimethylformamide in S1 was 0.5 g / mL.

[0094] The mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is 15:0.04:0.03.

[0095] The reaction temperature was maintained at 85°C in S2.

[0096] In S2, the ratio of ethyl acrylate to polylactic acid is 0.3 mL of ethyl acrylate per 1 g of polylactic acid; the ratio of butyl acrylate to polylactic acid is 0.1 mL of butyl acrylate per 1 g of polylactic acid.

[0097] The mass ratio of thioglycolic acid to polylactic acid in S2 is 0.0025:1.

[0098] The usage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.04 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; the usage mass ratio of triethylamine to polylactic acid is 0.004:1.

[0099] The amount of acetone used in S5 is 10 times the mass of grafted polylactic acid.

[0100] The mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is 0.05:1.

[0101] The concentration of the dilute sulfuric acid solution in S5 is 0.5 mol / L; the amount used is 15 vol% of the volume of acetone.

[0102] The heating and stirring reaction in S5 is carried out at a temperature of 70° C. for 7 hours.

[0103] The amount of polycaprolactone in S7 is 10 wt % of the modified polylactic acid.

[0104] The auxiliary agents in S7 include 2 wt % of phthalate modified polylactic acid and 0.2 wt % of calcium stearate modified polylactic acid.

[0105] Example 3 A hot air preparation method for a high-permeability and high-strength polylactic acid composite non-woven fabric:

[0106] S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well;

[0107] S2, maintaining the reaction temperature and continuing stirring, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction;

[0108] S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction;

[0109] S4, after the reaction is completed, the grafted polylactic acid is separated;

[0110] S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react;

[0111] S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid;

[0112] S7, taking the obtained modified polylactic acid, polycaprolactone, and additives and mixing them to obtain a spinning material;

[0113] S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0114] S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0115] In S8, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0116] The wire bundle spacing of S8 is 5mm, and the wire bundle tension is 1.5cN; the laying speed of the web is 20m / min, the laying angle is 50°, and the number of laying layers is 5.

[0117] In S9, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0118] The stirring and dissolving in S1 is carried out at 70°C.

[0119] The concentration of polylactic acid in dimethylformamide in S1 was 0.4 g / mL.

[0120] The mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is 10:0.04:0.03.

[0121] The reaction temperature was maintained at 80°C in S2.

[0122] In S2, the ratio of ethyl acrylate to polylactic acid is 0.2 mL of ethyl acrylate per 1 g of polylactic acid; the ratio of butyl acrylate to polylactic acid is 0.08 mL of butyl acrylate per 1 g of polylactic acid.

[0123] The mass ratio of thioglycolic acid to polylactic acid in S2 is 0.0020:1.

[0124] The usage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.03 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; the usage mass ratio of triethylamine to polylactic acid is 0.0030:1.

[0125] The amount of acetone used in S5 is 10 times the mass of grafted polylactic acid.

[0126] The mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is 0.03:1.

[0127] The concentration of the dilute sulfuric acid solution in S5 is 0.5 mol / L; the amount used is 15 vol% of the volume of acetone.

[0128] The heating and stirring reaction in S5 is carried out at a temperature of 70° C. for 3 hours.

[0129] The amount of polycaprolactone in S7 is 10 wt % of the modified polylactic acid.

[0130] The auxiliary agents in S7 include 2 wt % of phthalate modified polylactic acid and 0.2 wt % of calcium stearate modified polylactic acid.

[0131] Example 4 A hot air preparation method for a high-permeability and high-strength polylactic acid composite non-woven fabric:

[0132] S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well;

[0133] S2, maintaining the reaction temperature and continuing stirring, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction;

[0134] S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction;

[0135] S4, after the reaction is completed, the grafted polylactic acid is separated;

[0136] S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react;

[0137] S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid;

[0138] S7, taking the obtained modified polylactic acid, polycaprolactone, and additives and mixing them to obtain a spinning material;

[0139] S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0140] S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0141] In S8, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0142] The wire bundle spacing of S8 is 5mm, and the wire bundle tension is 1.5cN; the laying speed of the web is 20m / min, the laying angle is 50°, and the number of laying layers is 5.

[0143] In S9, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0144] The stirring and dissolving in S1 is carried out at 70°C.

[0145] The concentration of polylactic acid in dimethylformamide in S1 was 0.4 g / mL.

[0146] The mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is 10:0.04:0.03.

[0147] The reaction temperature was maintained at 80°C in S2.

[0148] In S2, the ratio of ethyl acrylate to polylactic acid is 0.2 mL of ethyl acrylate per 1 g of polylactic acid; the ratio of butyl acrylate to polylactic acid is 0.08 mL of butyl acrylate per 1 g of polylactic acid.

[0149] The mass ratio of thioglycolic acid to polylactic acid in S2 is 0.0020:1.

[0150] The usage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.03 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; the usage mass ratio of triethylamine to polylactic acid is 0.0030:1.

[0151] The amount of acetone used in S5 is 10 times the mass of grafted polylactic acid.

[0152] The mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is 0.03:1.

[0153] The concentration of the dilute sulfuric acid solution in S5 is 0.5 mol / L; the amount used is 15 vol% of the volume of acetone.

[0154] The heating and stirring reaction in S5 is carried out at a temperature of 70° C. for 3 hours.

[0155] The amount of polycaprolactone in S7 is 12 wt % of the modified polylactic acid.

[0156] The auxiliary agents in S7 include 2 wt % of phthalate modified polylactic acid and 0.2 wt % of calcium stearate modified polylactic acid.

[0157] Comparative Example 1 A hot air preparation method for polylactic acid composite non-woven fabric (polylactic acid is not modified):

[0158] S1, taking polylactic acid, polycaprolactone, and an additive and mixing them to obtain a spinning material;

[0159] S2, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0160] S3, laying the obtained fibers through swinging wire, and subjecting the obtained fiber web to hot air treatment to shape into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0161] In S2, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0162] The wire bundle spacing of S2 is 5 mm, and the wire bundle tension is 1.5 cN; the laying speed of the web is 20 m / min, the laying angle is 50°, and the number of laying layers is 5.

[0163] In S3, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0164] The amount of polycaprolactone in S1 is 12 wt % of the modified polylactic acid.

[0165] The auxiliary agents in S1 include 2 wt % of polylactic acid phthalate and 0.2 wt % of polylactic acid calcium stearate.

[0166] Comparative Example 2 A hot air preparation method for polylactic acid composite non-woven fabric (without adding polycaprolactone):

[0167] S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well;

[0168] S2, maintaining the reaction temperature and continuing stirring, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction;

[0169] S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction;

[0170] S4, after the reaction is completed, the grafted polylactic acid is separated;

[0171] S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react;

[0172] S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid;

[0173] S7, taking the obtained modified polylactic acid and an auxiliary agent and mixing them to obtain a spinning material;

[0174] S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0175] S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0176] In S8, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0177] The wire bundle spacing of S8 is 5mm, and the wire bundle tension is 1.5cN; the laying speed of the web is 20m / min, the laying angle is 50°, and the number of laying layers is 5.

[0178] In S9, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0179] The stirring and dissolving in S1 is carried out at 70°C.

[0180] The concentration of polylactic acid in dimethylformamide in S1 was 0.4 g / mL.

[0181] The mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is 10:0.04:0.03.

[0182] The reaction temperature was maintained at 80°C in S2.

[0183] In S2, the ratio of ethyl acrylate to polylactic acid is 0.2 mL of ethyl acrylate per 1 g of polylactic acid; the ratio of butyl acrylate to polylactic acid is 0.08 mL of butyl acrylate per 1 g of polylactic acid.

[0184] The mass ratio of thioglycolic acid to polylactic acid in S2 is 0.0020:1.

[0185] The usage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.03 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; the usage mass ratio of triethylamine to polylactic acid is 0.0030:1.

[0186] The amount of acetone used in S5 is 10 times the mass of grafted polylactic acid.

[0187] The mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is 0.03:1.

[0188] The concentration of the dilute sulfuric acid solution in S5 is 0.5 mol / L; the amount used is 15 vol% of the volume of acetone.

[0189] The heating and stirring reaction in S5 is carried out at a temperature of 70° C. for 3 hours.

[0190] The auxiliary agents in S7 include 2 wt % of phthalate modified polylactic acid and 0.2 wt % of calcium stearate modified polylactic acid.

[0191] Comparative Example 3 A hot air preparation method for polylactic acid composite non-woven fabric (polylactic acid is not modified and polycaprolactone is not added):

[0192] S1, taking polylactic acid and an additive and mixing them to obtain a spinning material;

[0193] S2, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers;

[0194] S3, laying the obtained fibers through swinging wire, and subjecting the obtained fiber web to hot air treatment to shape into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

[0195] In S2, the melting temperature is 180°C, the spinning temperature is 190°C, the winding speed is 800m / min; the drawing temperature is 70°C, and the multiple is 2.2 times.

[0196] The wire bundle spacing of S2 is 5 mm, and the wire bundle tension is 1.5 cN; the laying speed of the web is 20 m / min, the laying angle is 50°, and the number of laying layers is 5.

[0197] In S3, the hot air temperature is 100°C, the hot air speed is 4m / s, and the hot air combing time is 30s.

[0198] The auxiliary agents in S1 include 2 wt % of polylactic acid phthalate and 0.2 wt % of polylactic acid calcium stearate.

[0199] Performance testing:

[0200] Air permeability test: Standard number: GB / T 5453-1977 "Determination of air permeability of textile fabrics"; Test operation: Randomly cut 10 samples with a diameter of 50mm from the non-woven fabric sample. Clamp one of the samples in the air permeability tester to ensure that the sample is flat, not deformed, and the two sides of the sample are well sealed. Set the pressure difference value on both sides of the sample to 100Pa, and adjust the pressure control valve to achieve this pressure difference. When the pressure difference value stabilizes and reaches the set value, the equipment will automatically display the gas flow rate passing through the sample at this time. Take the average value of 10 samples.

[0201] Strength test: Standard number: Refer to GB / T 24218.3-2010 "Test methods for textile nonwovens Part 3: Determination of breaking strength and breaking elongation"; Test operation: Cut a specimen of specified size from the nonwoven fabric, usually in a rectangular shape. Use a tensile testing machine to fix the specimen between the clamps to ensure that the specimen is flat and tension-free. Stretch the specimen at a constant speed until it breaks. Record the maximum force and elongation when the specimen breaks.

[0202] The samples obtained in all the above embodiments and comparative examples were subjected to the above tests, and the results obtained are shown in Table 1.

[0203] Table 1 Product permeability and strength test parameters

[0204] sample <![CDATA[Air permeability m 3 / m 2 ·s]]> Breaking strength N Elongation at break % Example 1 321.5 3818 45.3 Example 2 326.1 3832 48.1 Example 3 324.8 3813 47.6 Example 4 319.6 3857 45.9 Comparative Example 1 322.8 969 19.0 Comparative Example 2 326.3 2781 34.2 Comparative Example 3 317.9 981 19.6

[0205] It can be seen from the experimental data that when the steps of swinging, laying, needling, hot air combing, etc. are the same, the air permeability of the obtained non-woven fabric is almost the same, which meets the use requirements. On this basis, the modified polylactic acid provided by the present invention can greatly improve the breaking strength and breaking elongation of the prepared non-woven fabric. In addition, the polycaprolactone added in step seven is usually used to adjust the elasticity of the fiber in our previous research and development. Past data show that the addition of polycaprolactone usually does not have a significant effect on the strength of polylactic acid fibers and the strength of non-woven fabrics. When the amount of polycaprolactone added exceeds 25wt% of polylactic acid, the strength of the fiber or non-woven fabric usually decreases significantly. In the present application, it is obvious that there is a certain interaction between the addition of polycaprolactone and the modified polylactic acid provided by the present invention, resulting in a synergistic effect that significantly improves the strength of the final product.

[0206] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0207] The present invention and its implementation methods are described above, which is not restrictive. What is shown is only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A hot air preparation method for high-permeability and high-strength polylactic acid composite non-woven fabric, characterized in that: The following steps are involved: S1, taking polylactic acid and stirring and dissolving it in dimethylformamide, adding potassium persulfate and sodium bisulfite and mixing well; S2, maintaining the reaction temperature and stirring continuously, under nitrogen protection, slowly adding ethyl acrylate and butyl acrylate at the same time, gradually adding thioglycolic acid, and continuing the reaction; S3, after adding trimethylolpropane triacrylate, add triethylamine and continue the reaction; S4, after the reaction is completed, the grafted polylactic acid is separated; S5, the obtained grafted polylactic acid is dissolved in acetone with stirring, tetraethylammonium bromide is added to dissolve, and a dilute sulfuric acid solution is slowly added dropwise, and the mixture is heated and stirred to react; S6, cooling after the reaction is completed, separating and obtaining modified polylactic acid; S7, taking the obtained modified polylactic acid, polycaprolactone, and an auxiliary agent and mixing them to obtain a spinning material; S8, adding the obtained spinning material into a screw extruder for melting, spinning and winding, drawing, and drying to obtain fibers; S9, laying the obtained fibers through swinging wires, and subjecting the obtained fiber web to hot air treatment to shape it into cloth, thereby obtaining a polylactic acid composite non-woven fabric.

2. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: In S8, the melting temperature is 180-200°C, the spinning temperature is 190-230°C, the winding speed is 800-1000m / min; the drawing temperature is 70-90°C, and the multiple is 2.2-3.5 times.

3. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The wire bundle spacing of the swing wire in S8 is 5-8mm, and the wire bundle tension is 1.5-2.5cN; the laying speed of the web is 20-50m / min, the laying angle is 50-80°, excluding 60°, and the number of laying layers is 5-10.

4. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: In S9, the hot air temperature is 100-130℃, the hot air speed is 4-8m / s, and the hot air combing time is 30-50s.

5. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The stirring and dissolving in S1 is carried out at 70-75°C.

6. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The concentration of polylactic acid in S1 in dimethylformamide is 0.3-0.5 g / mL; the mass ratio of polylactic acid, potassium persulfate and sodium bisulfite in S1 is (10-15):(0.04-0.08):(0.03-0.06).

7. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The reaction temperature is maintained at 80-85°C in S2.

8. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The dosage ratio of ethyl acrylate to polylactic acid in S2 is 0.15-0.3 mL of ethyl acrylate per 1 g of polylactic acid; the dosage ratio of butyl acrylate to polylactic acid is 0.05-0.1 mL of butyl acrylate per 1 g of polylactic acid; the mass ratio of thioglycolic acid to polylactic acid in S2 is (0.0015-0.0025):

1.

9. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The dosage ratio of trimethylolpropane triacrylate to polylactic acid in S3 is 0.02-0.04 mL of trimethylolpropane triacrylate per 1 g of polylactic acid; the dosage mass ratio of triethylamine to polylactic acid is (0.0025-0.004):

1.

10. The hot air preparation method of high-permeability and high-strength polylactic acid composite non-woven fabric according to claim 1, characterized in that: The amount of acetone in S5 is 5-10 times the mass of the grafted polylactic acid; the mass ratio of tetraethylammonium bromide to grafted polylactic acid in S5 is (0.01-0.05):1; the concentration of the dilute sulfuric acid solution in S5 is 0.5-1.5 mol / L; the amount is 15-25 vol% of the volume of acetone; the heating and stirring reaction in S5 is at a temperature of 50-70°C and a time of 3-7 hours.

Citation Information

Patent Citations

  • Preparation method of elastic polylactic acid fiber

    CN103255503A

  • Modified polylactic acid non-woven fabric as well as preparation method and application thereof

    CN113862903A

  • High-strength polylactic acid composite fiber and preparation method thereof

    CN118461176A

  • Biodegradable resin composition

    JP2004189770A

Cited By

  • Non-woven fabric processing technology control method and system

    CN119392445A

  • High-performance biodegradable nonwoven fabric and preparation method thereof

    CN122669516A