Preparation method and application of high-breathability antibacterial ultraviolet-proof fabric

Through the application of modified bimini quaternary ammonium salt finishing agent in polyester fabrics, the shortcomings of the fabric in terms of UV resistance, antibacterial and breathable properties are solved, and efficient UV absorption and bacterial inhibition are achieved, which significantly improves the health function of the fabric.

CN118979382AInactive Publication Date: 2024-11-19PUNING SHENGDA TEXTILE CO LTD

Patent Information

Application Number
CN202411065359.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fabrics have shortcomings in their anti-UV, antibacterial and breathable properties, and cannot effectively protect human health, especially in the ultraviolet radiation and bacterial infections in the sun.

Method used

Using modified bimini quaternary ammonium salt finishing agent, a series of chemical reactions are prepared to obtain a bimini quaternary ammonium salt finishing agent containing haloamine and quaternary ammonium salt structure, and applied it to polyester fabrics. It is organized by modified bimini quaternary ammonium salt. The structure of the agent improves the antibacterial properties and UV absorption properties of the fabric while maintaining high breathability.

Benefits of technology

The prepared high-breathable antibacterial and ultraviolet-resistant fabrics show excellent antibacterial properties, ultraviolet-resistant properties and breathable properties, which can effectively shield ultraviolet rays of 280-340nm and significantly improve the inhibitory effect on bacteria.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979199110000021
    Figure BDA0004979199110000021
  • Figure BDA0004979199110000022
    Figure BDA0004979199110000022
  • Figure BDA0004979199110000031
    Figure BDA0004979199110000031
Patent Text Reader

Abstract

The invention relates to the technical field of fabrics, and discloses a preparation method and application of a high-breathability antibacterial ultraviolet-proof fabric. Phenolic hydroxyl groups of 2, 4-dihydroxybenzophenone react with alkenyl groups in allylsuccinic anhydride to prepare an intermediate 1, the intermediate 1 reacts with aminoethyl hydantoin and tris (2-aminoethyl) amine to prepare a high-breathability antibacterial ultraviolet-proof fabric, and then the high-breathability antibacterial ultraviolet-proof fabric is obtained. The preparation method comprises the following steps: carrying out two amidation reactions to prepare an intermediate 3, carrying out a quaternization reaction on the intermediate 3 and 1, 6-dibromohexane to obtain a modified gemini quaternary ammonium salt finishing agent, chlorinating the modified gemini quaternary ammonium salt finishing agent, and applying the chlorinated modified gemini quaternary ammonium salt finishing agent to the polyester fabric, so that the prepared fabric has excellent ultraviolet resistance, antibacterial property and air permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabrics, and in particular to a preparation method and application of a highly breathable, antibacterial and ultraviolet-proof fabric. Background Art

[0002] With the advancement of science and technology, in addition to meeting the basic requirements of warmth retention and comfort performance, people have higher and higher functional requirements for textiles, such as radiation protection, radiation protection, and UV resistance. The ultraviolet rays in the sun can cause damage to human skin, and in severe cases can even cause skin cancer. Therefore, certain methods are used to shield ultraviolet radiation to reduce its damage to the skin. At the same time, the fabrics worn are prone to produce Escherichia coli, Staphylococcus aureus, etc. in the hidden parts of the skin, affecting the physiological health of the human body. Therefore, it is necessary to improve the anti-ultraviolet performance, breathability and antibacterial performance of the fabric.

[0003] Compared with other UV absorbers, benzophenone UV absorbers have the characteristics of simple structure, good stability and low price, and are widely used in the anti-ultraviolet properties of various fabrics. Quaternary ammonium surfactants all contain an ionized nitrogen atom and are widely used in fabric conditioners, pesticides, etc. They have good antibacterial properties. The antibacterial mechanism is: quaternary ammonium salts dissociate into quaternary ammonium cations with positive charges in aqueous solution, and their nitrogen ions can be adsorbed onto the negatively charged bacterial cell walls, which can destroy the cell membrane, denature proteins, and hinder the replication and reproduction of DNA, thereby achieving a good antibacterial effect. Halamine antibacterial agents have the advantages of broad-spectrum antibacterial, high-efficiency antibacterial, environmentally friendly, and good renewability, and will not cause bacterial resistance. Halamine antibacterial textiles meet people's needs for healthy living and have good market prospects. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing a highly breathable, antibacterial and UV-proof fabric and its application. The prepared polyester fabric has excellent antibacterial, UV-proof and breathable properties.

[0006] (II) Technical solution

[0007] A preparation method of a highly breathable, antibacterial and ultraviolet-proof fabric, comprising the following steps: adding a modified gemini quaternary ammonium salt finishing agent to deionized water, stirring and dispersing, then adding sodium hypochlorite with a mass fraction of 4-10% and sulfuric acid with a mass fraction of 0.2-0.6 mol / L to the water to adjust the pH value to 7-8, stirring and reacting for 3-6 hours at room temperature, washing with deionized water, drying, adding the modified gemini quaternary ammonium salt finishing agent to deionized water to prepare a 20-50% solution, adding a 10 cm×20 cm polyester fabric to the solution with a bath ratio of 1:30-50, adjusting the pH value to 8-10 with sodium hydroxide, impregnating and reacting at 30-40°C for 30-60 minutes, heating to 80-90°C, adding sodium chloride with a mass concentration of 10-30 g / L to the water, continuing to react for 30-60 minutes, heating to room temperature, drying, washing with water, soaping, and washing with water to obtain the highly breathable, antibacterial and ultraviolet-proof fabric.

[0008] Preferably, the preparation method of the modified gemini quaternary ammonium salt finishing agent is:

[0009] (1) Under nitrogen conditions, 2,4-dihydroxybenzophenone is added to an ethanol solvent, stirred and dispersed, and then allyl succinic anhydride is added thereto, reacted at 55-70° C. for 5-12 hours. After the reaction is completed, the mixture is rotary evaporated, washed with deionized water, and dried to obtain an intermediate 1, the reaction formula of which is:

[0010]

[0011] (2) Under nitrogen conditions, intermediate 1 is added to N,N-dimethylformamide solvent, stirred and dispersed, and then aminoethyl hydantoin is added thereto. The mixture is stirred and reacted at room temperature for 3-6 hours. After the reaction is completed, the mixture is filtered, washed with deionized water, and dried to obtain intermediate 2, whose reaction formula is:

[0012]

[0013] (3) Under nitrogen conditions, intermediate 2, tris(2-aminoethyl)amine, and dicyclohexylcarbodiimide (DCC) were added to N,N-dimethylformamide solvent, stirred and dispersed, and stirred and reacted at room temperature for 12-24 hours. After the reaction was completed, the filtrate was filtered under reduced pressure, and the filtrate was collected and dried to obtain intermediate 3, whose reaction formula is:

[0014] (4) Adding intermediate 3 and 1,6-dibromohexane to an ethanol solvent, reacting at 100-120° C. for 40-72 hours, cooling to room temperature after the reaction, filtering, and drying to obtain a modified gemini quaternary ammonium salt finishing agent, the reaction formula of which is:

[0015] Preferably, in step (1), the molar ratio of 2,4-dihydroxybenzophenone to allyl succinic anhydride is 1:1.5-2.

[0016] Preferably, in step (2), the molar ratio of intermediate 1 to aminoethylhydantoin is 1:0.8-1.2.

[0017] Preferably, in step (3), the molar ratio of intermediate 2, tris(2-aminoethyl)amine, and DCC is 3-4:1:6-10.

[0018] Preferably, in step (4), the molar ratio of the intermediate 3 to 1,6-dibromohexane is 2-2.5:1.

[0019] Preferably, the highly breathable, antibacterial and UV-proof fabric can be used in the field of clothing fabrics.

[0020] (III) Beneficial technical effects

[0021] The invention uses 2,4-dihydroxybenzophenone, allyl succinic anhydride, aminoethyl hydantoin, tris(2-aminoethyl)amine, 1,6-dibromohexane and the like as raw materials, and prepares a modified gemini quaternary ammonium salt finishing agent through a series of reactions. The modified gemini quaternary ammonium salt finishing agent prepared by the invention has a novel structure, and is applied to polyester fabrics to prepare highly breathable, antibacterial and ultraviolet-proof fabrics.

[0022] The gemini quaternary ammonium salt finishing agent prepared by the present invention contains a halamine structure and a quaternary ammonium salt structure, and has better antibacterial performance than a single halamine structure and a single quaternary ammonium salt structure. The gemini quaternary ammonium salt finishing agent is applied to polyester fabrics to improve the antibacterial performance of the polyester fabrics. The gemini quaternary ammonium salt finishing agent prepared by the present invention also contains a benzophenone structure, and has better absorption performance for ultraviolet rays of 280-340nm. The gemini quaternary ammonium salt finishing agent is applied to polyester fabrics to improve the anti-ultraviolet performance of the polyester fabrics. Tests have confirmed that the fabrics prepared by the present invention have excellent anti-ultraviolet performance, antibacterial performance and air permeability. DETAILED DESCRIPTION

[0023] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0024] Example 1

[0025] (1) Under nitrogen conditions, 0.4 mol of 2,4-dihydroxybenzophenone was added to 200 mL of ethanol solvent, stirred and dispersed, and then 0.6 mol of allyl succinic anhydride was added thereto, and the mixture was reacted at 60° C. for 10 h. After the reaction was completed, the mixture was rotary evaporated, washed with deionized water, and dried to obtain intermediate 1.

[0026] (2) Under nitrogen conditions, 0.1 mol of intermediate 1 was added to 200 mL of N,N-dimethylformamide solvent and stirred for dispersion. Then, 0.09 mol of aminoethylhydantoin was added thereto and stirred for reaction at room temperature for 5 h. After the reaction was completed, the mixture was filtered, washed with deionized water, and dried to obtain intermediate 2.

[0027] (3) Under nitrogen conditions, 0.03 mol of intermediate 2, 0.01 mol of tris(2-aminoethyl)amine, and 0.08 mol of DCC were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and stirred and reacted at room temperature for 20 h. After the reaction was completed, the filtrate was filtered under reduced pressure, collected, and dried to obtain intermediate 3.

[0028] (4) 0.24 mol of intermediate 3 and 0.1 mol of 1,6-dibromohexane were added to 200 mL of ethanol solvent and reacted at 120° C. for 40 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and dried to obtain a modified gemini quaternary ammonium salt finishing agent.

[0029] (5) The modified gemini quaternary ammonium salt finishing agent is added to deionized water, stirred and dispersed, and then 10% sodium hypochlorite and 0.2 mol / L sulfuric acid are added thereto to adjust the pH to 8. The mixture is stirred and reacted at room temperature for 6 hours. After completion, the mixture is washed with deionized water and dried. The mixture is added to deionized water to form a 20% solution. A 10 cm × 20 cm polyester fabric is added to the solution with a bath ratio of 1:30. Sodium hydroxide is used to adjust the pH to 10. The mixture is immersed at 35° C. for 60 minutes, heated to 85° C., and sodium chloride with a mass concentration of 20 g / L is added thereto. The mixture is reacted for 40 minutes. The mixture is cooled to room temperature, dried, washed with water, soaped, and washed with water to obtain a highly breathable, antibacterial, and UV-resistant fabric.

[0030] Example 2

[0031] (1) Under nitrogen conditions, 0.4 mol of 2,4-dihydroxybenzophenone was added to 200 mL of ethanol solvent, stirred and dispersed, and then 0.8 mol of allyl succinic anhydride was added thereto, and the mixture was reacted at 70° C. for 5 h. After the reaction was completed, the mixture was rotary evaporated, washed with deionized water, and dried to obtain intermediate 1.

[0032] (2) Under nitrogen conditions, 0.1 mol of intermediate 1 was added to 200 mL of N,N-dimethylformamide solvent and stirred for dispersion. Then, 0.12 mol of aminoethylhydantoin was added thereto and stirred for reaction at room temperature for 5 h. After the reaction was completed, the mixture was filtered, washed with deionized water, and dried to obtain intermediate 2.

[0033] (3) Under nitrogen conditions, 0.03 mol of intermediate 2, 0.01 mol of tris(2-aminoethyl)amine, and 0.1 mol of DCC were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and stirred for reaction at room temperature for 22 h. After the reaction was completed, the filtrate was filtered under reduced pressure, collected, and dried to obtain intermediate 3.

[0034] (4) 0.25 mol of intermediate 3 and 0.1 mol of 1,6-dibromohexane were added to 200 mL of ethanol solvent and reacted at 100° C. for 48 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and dried to obtain a modified gemini quaternary ammonium salt finishing agent.

[0035] (5) The modified gemini quaternary ammonium salt finishing agent is added to deionized water, stirred and dispersed, and then 4% sodium hypochlorite and 0.6 mol / L sulfuric acid are added thereto to adjust the pH to 7. The mixture is stirred and reacted at room temperature for 4 hours. After completion, the mixture is washed with deionized water and dried. The mixture is added to deionized water to prepare a 30% solution. A 10 cm × 20 cm polyester fabric is added to the solution with a bath ratio of 1:50. The pH is adjusted to 8 with sodium hydroxide. The mixture is immersed at 40°C for 40 minutes, heated to 80°C, and sodium chloride with a mass concentration of 30 g / L is added thereto. The mixture is reacted for 50 minutes. The mixture is cooled to room temperature, dried, washed with water, soaped, and washed with water to obtain a highly breathable, antibacterial, and UV-resistant fabric.

[0036] Example 3

[0037] (1) Under nitrogen conditions, 0.4 mol of 2,4-dihydroxybenzophenone was added to 200 mL of ethanol solvent, stirred and dispersed, and then 0.7 mol of allyl succinic anhydride was added thereto, and the mixture was reacted at 55° C. for 12 h. After the reaction was completed, the mixture was rotary evaporated, washed with deionized water, and dried to obtain intermediate 1.

[0038] (2) Under nitrogen conditions, 0.1 mol of intermediate 1 was added to 200 mL of N,N-dimethylformamide solvent and stirred for dispersion. Then, 0.1 mol of aminoethylhydantoin was added thereto and stirred for reaction at room temperature for 3 h. After the reaction was completed, the mixture was filtered, washed with deionized water, and dried to obtain intermediate 2.

[0039] (3) Under nitrogen conditions, 0.03 mol of intermediate 2, 0.01 mol of tris(2-aminoethyl)amine, and 0.06 mol of DCC were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and stirred and reacted at room temperature for 20 h. After the reaction was completed, the filtrate was filtered under reduced pressure and collected and dried to obtain intermediate 3.

[0040] (4) 0.2 mol of intermediate 3 and 0.1 mol of 1,6-dibromohexane were added to 200 mL of ethanol solvent and reacted at 110° C. for 72 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and dried to obtain a modified gemini quaternary ammonium salt finishing agent.

[0041] (5) The modified gemini quaternary ammonium salt finishing agent is added to deionized water, stirred and dispersed, and then 5% sodium hypochlorite and 0.4 mol / L sulfuric acid are added thereto to adjust the pH to 8. The mixture is stirred and reacted at room temperature for 3 hours. After completion, the mixture is washed with deionized water and dried. The mixture is added to deionized water to form a 40% solution. A 10 cm × 20 cm polyester fabric is added to the solution with a bath ratio of 1:50. Sodium hydroxide is used to adjust the pH to 9. The mixture is immersed at 30°C for 30 minutes, heated to 90°C, and sodium chloride with a mass concentration of 10 g / L is added thereto. The mixture is reacted for 60 minutes. The mixture is cooled to room temperature, dried, washed with water, soaped, and washed with water to obtain a highly breathable, antibacterial, and UV-resistant fabric.

[0042] Example 4

[0043] (1) Under nitrogen conditions, 0.4 mol of 2,4-dihydroxybenzophenone was added to 200 mL of ethanol solvent, stirred and dispersed, and then 0.7 mol of allyl succinic anhydride was added thereto, and the mixture was reacted at 60° C. for 8 h. After the reaction was completed, the mixture was rotary evaporated, washed with deionized water, and dried to obtain intermediate 1.

[0044] (2) Under nitrogen conditions, 0.1 mol of intermediate 1 was added to 200 mL of N,N-dimethylformamide solvent and stirred for dispersion. Then, 0.12 mol of aminoethylhydantoin was added thereto and stirred for reaction at room temperature for 6 h. After the reaction was completed, the mixture was filtered, washed with deionized water, and dried to obtain intermediate 2.

[0045] (3) Under nitrogen conditions, 0.04 mol of intermediate 2, 0.01 mol of tris(2-aminoethyl)amine, and 0.1 mol of DCC were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and stirred for reaction at room temperature for 12 h. After the reaction was completed, the filtrate was filtered under reduced pressure, collected, and dried to obtain intermediate 3.

[0046] (4) 0.24 mol of intermediate 3 and 0.1 mol of 1,6-dibromohexane were added to 200 mL of ethanol solvent and reacted at 110° C. for 48 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and dried to obtain a modified gemini quaternary ammonium salt finishing agent.

[0047] (5) The modified gemini quaternary ammonium salt finishing agent is added to deionized water, stirred and dispersed, and then 6% sodium hypochlorite and 0.5 mol / L sulfuric acid are added thereto to adjust the pH to 7. The mixture is stirred and reacted at room temperature for 6 hours. After completion, the mixture is washed with deionized water and dried. The mixture is added to deionized water to prepare a 45% solution. A 10 cm × 20 cm polyester fabric is added to the solution with a bath ratio of 1:40. Sodium hydroxide is used to adjust the pH to 9. The mixture is immersed at 35°C for 50 minutes, heated to 85°C, and sodium chloride with a mass concentration of 20 g / L is added thereto. The mixture is reacted for 30 minutes. The mixture is cooled to room temperature, dried, washed with water, soaped, and washed with water to obtain a highly breathable, antibacterial, and UV-resistant fabric.

[0048] Example 5

[0049] (1) Under nitrogen conditions, 0.4 mol of 2,4-dihydroxybenzophenone was added to 200 mL of ethanol solvent, stirred and dispersed, and then 0.7 mol of allyl succinic anhydride was added thereto, and the mixture was reacted at 65° C. for 10 h. After the reaction was completed, the mixture was rotary evaporated, washed with deionized water, and dried to obtain intermediate 1.

[0050] (2) Under nitrogen conditions, 0.1 mol of intermediate 1 was added to 200 mL of N,N-dimethylformamide solvent and stirred for dispersion. Then, 0.08 mol of aminoethylhydantoin was added thereto and stirred for reaction at room temperature for 5 h. After the reaction was completed, the mixture was filtered, washed with deionized water, and dried to obtain intermediate 2.

[0051] (3) Under nitrogen conditions, 0.03 mol of intermediate 2, 0.01 mol of tris(2-aminoethyl)amine, and 0.08 mol of DCC were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and stirred and reacted at room temperature for 24 h. After the reaction was completed, the filtrate was filtered under reduced pressure and collected and dried to obtain intermediate 3.

[0052] (4) 0.24 mol of intermediate 3 and 0.1 mol of 1,6-dibromohexane were added to 200 mL of ethanol solvent and reacted at 110° C. for 60 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and dried to obtain a modified gemini quaternary ammonium salt finishing agent.

[0053] (5) The modified gemini quaternary ammonium salt finishing agent is added to deionized water, stirred and dispersed, and then 8% sodium hypochlorite and 0.4 mol / L sulfuric acid are added thereto to adjust the pH to 8. The mixture is stirred and reacted at room temperature for 4 hours. After completion, the mixture is washed with deionized water and dried. The mixture is added to deionized water to prepare a 50% solution. A 10 cm × 20 cm polyester fabric is added to the solution with a bath ratio of 1:40. Sodium hydroxide is used to adjust the pH to 9. The mixture is immersed at 35°C for 50 minutes, heated to 85°C, and sodium chloride with a mass concentration of 10 g / L is added thereto. The mixture is reacted for 60 minutes. The mixture is cooled to room temperature, dried, washed with water, soaped, and washed with water to obtain a highly breathable, antibacterial, and UV-resistant fabric.

[0054] Comparative Example 1

[0055] The difference between this comparative example and Example 1 is that in step (5), intermediate 2 is used instead of the modified gemini quaternary ammonium salt finishing agent.

[0056] Comparative Example 2

[0057] The difference between this comparative example and Example 1 is that in step (5), no modified gemini quaternary ammonium salt finishing agent is contained.

[0058] Refer to GB / T18830-2009 and use the textile UV protection tester to test the UV protection factor (UPF value) of the fabric.

[0059] Refer to GB / T5453-1997 and use a fabric air permeability tester to test the air permeability of the fabric.

[0060] Table 1: Test results of UV resistance and air permeability of various embodiments and comparative examples

[0061] UPF value Air permeability / (L / mm·s) Example 1 68.17 1430 Example 2 89.75 1468 Example 3 104.30 1521 Example 4 129.27 1548 Example 5 118.04 1493 Comparative Example 1 70.58 1416 Comparative Example 2 40.06 1306

[0062] The larger the UPF value, the better the anti-ultraviolet performance, and the larger the air permeability, the better the air permeability. It can be seen from the table that the fabric prepared by the present invention has good anti-ultraviolet performance and air permeability.

[0063] With reference to GB / T20944.3-2008, the antibacterial properties of the fabric were tested. The test bacteria were Staphylococcus aureus and Escherichia coli. The inhibition rate (%) = (control sample live bacteria (CFU / mL) - sample live bacteria (CFU / mL)) / control sample live bacteria (CFU / mL).

[0064] Table 2: Antibacterial test results of various embodiments and comparative examples

[0065]

[0066]

[0067] It can be seen from the table that the fabric prepared by the present invention has excellent antibacterial properties.

[0068] The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions also belong to the scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. A method for preparing a highly breathable, antibacterial and UV-proof fabric. It is characterized in that The preparation method comprises the following steps: adding a modified gemini quaternary ammonium salt finishing agent into deionized water, stirring and dispersing the mixture, adding sodium hypochlorite and 0.2-0.6 mol / L sulfuric acid thereto to adjust the pH value to 7-8, stirring and reacting the mixture for 3-6 hours at room temperature, washing the mixture with deionized water, drying the mixture, adding the modified gemini quaternary ammonium salt finishing agent into deionized water to prepare a 20-50% solution, adding a 10 cm×20 cm polyester fabric into the solution with a bath ratio of 1:30-50, adjusting the pH value to 8-10 with sodium hydroxide, impregnating the mixture at 30-40°C for reaction for 30-60 minutes, heating the mixture to 80-90°C, adding sodium chloride thereto, continuing the reaction for 30-60 minutes, heating the mixture to room temperature, drying the mixture, washing the mixture with water, soaping the mixture, and washing the mixture with water to obtain a highly breathable, antibacterial, and UV-resistant fabric.

2. The method for preparing the highly breathable, antibacterial and UV-proof fabric according to claim 1, It is characterized in that The mass fraction of the sodium hypochlorite is 4-10%; the mass concentration of the sodium chloride is 10-30 g / L.

3. The method for preparing the highly breathable, antibacterial and UV-proof fabric according to claim 1, It is characterized in that The preparation method of the modified gemini quaternary ammonium salt finishing agent is: (1) Under nitrogen conditions, 2,4-dihydroxybenzophenone is added to an ethanol solvent, stirred and dispersed, and then allyl succinic anhydride is added thereto, reacted at 55-70° C. for 5-12 hours. After the reaction is completed, the mixture is rotary evaporated, washed with deionized water, and dried to obtain an intermediate 1; (2) Under nitrogen conditions, the intermediate 1 is added to N,N-dimethylformamide solvent, stirred and dispersed, and then aminoethyl hydantoin is added thereto. The mixture is stirred and reacted at room temperature for 3-6 hours. After the reaction is completed, the mixture is filtered, washed with deionized water, and dried to obtain the intermediate 2; (3) Under nitrogen conditions, intermediate 2, tris(2-aminoethyl)amine, and DCC were added to N,N-dimethylformamide solvent, stirred and dispersed, and stirred at room temperature for 12-24 hours. After the reaction was completed, the filtrate was filtered under reduced pressure, and the filtrate was collected and dried to obtain intermediate 3; (4) Adding the intermediate 3 and 1,6-dibromohexane to an ethanol solvent, reacting at 100-120° C. for 40-72 hours, cooling to room temperature after the reaction, filtering, and drying to obtain a modified gemini quaternary ammonium salt finishing agent.

4. The method for preparing the highly breathable, antibacterial and UV-proof fabric according to claim 3, It is characterized in that In the step (1), the molar ratio of 2,4-dihydroxybenzophenone to allyl succinic anhydride is 1:1.5-2.

5. The method for preparing the highly breathable, antibacterial and UV-proof fabric according to claim 3, It is characterized in that In the step (2), the molar ratio of the intermediate 1 to aminoethylhydantoin is 1:0.8-1.

2.

6. The method for preparing the highly breathable, antibacterial and UV-proof fabric according to claim 3, It is characterized in that In the step (3), the molar ratio of intermediate 2, tris(2-aminoethyl)amine, and DCC is 3-4:1:6-10.

7. The method for preparing the highly breathable, antibacterial and UV-proof fabric according to claim 3, It is characterized in that In the step (4), the molar ratio of the intermediate 3 to 1,6-dibromohexane is 2-2.5:

1.

8. An application of the highly breathable, antibacterial and UV-proof fabric prepared by the preparation method according to claim 1, It is characterized in that The highly breathable, antibacterial and ultraviolet-proof fabric can be used in the field of clothing fabrics.

Citation Information

Patent Citations

  • Pyridine quaternary ammonium salt type halamine antibacterial agent and preparation method thereof

    CN104926787A

  • Halamine modified antibacterial cotton fabric and preparation method thereof

    CN112695522A

  • Anti-ultraviolet finishing agent and preparation method thereof

    CN113789656A

  • Finishing agent with antibacterial and anti-ultraviolet properties and method for finishing cotton fabric by adopting finishing agent

    CN113846484A

  • Preparation method and application of antistatic moisture-permeable polyester fabric

    CN116289204A