Experimental method for obtaining fatigue crack condition of blade foreign object damage front edge
By using a silicone rubber curing device on the aero engine blade for remodeling, combined with finite element method and three-dimensional modeling, the problems of low experimental efficiency and large test error in the small crack propagation research of blades are solved, and the external objects of the blade are realized before the damage of the blades is damaged. Efficient acquisition and simplified operation of edge fatigue cracks.
Patent Information
- Application Number
- CN202411193025.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-19
AI Technical Summary
In the research on small cracks in the aviation engine blades, there are problems such as low experimental efficiency, large test errors and equipment limitations in the research on small cracks of aero engine blades. Especially the geometric characteristics of the leading edge bending and twisting composite of the blades lead to difficulties in observation in situ, and the traditional silicone rubber compounding method is complicated to operate. And affect the test results.
The leading edge of the blade is reshaped by using the silicone rubber curing device, and the hazardous position and stress value are determined by the finite element method. The silicone rubber curing device is made using three-dimensional modeling, and the interrupt fatigue test is performed and the cracks on the recombinant silicone rubber are observed. , simplifies operation and improves efficiency.
It realizes efficient acquisition of fatigue cracks in the leading edge of the blade external objects damage, simplifies the operation process, improves the experimental efficiency, avoids errors caused by the disassembly of the test parts, and makes crack observation more convenient.
Smart Images

Figure CN118980594A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fatigue crack testing of aeroengine blades, and in particular to an experimental method for obtaining fatigue crack conditions of the leading edge of a blade damaged by foreign objects. Background Art
[0002] Studies have shown that the crack initiation and small crack growth stages of aircraft engine blades under high cycle fatigue loads exceed 90% of their total fatigue life. The study of the characteristics of the small crack growth stage of blades has important engineering significance. At present, the small crack observation techniques under laboratory conditions include in-situ optical microscope, in-situ scanning electron microscope, in-situ X-ray microphotography, interruption test SEM, interruption test cellulose acetate film replica, interruption test silicone rubber replica, etc.
[0003] High-resolution in-situ observation technology is the most advanced and accurate way to study the propagation of small cracks in materials, but this will be limited by the testing requirements of precision instruments and equipment, such as vacuum test environment, small test area, standard test samples, etc. For blade-like structural parts, the geometric characteristics of the leading edge bending and torsion determine that the focal plane cannot be kept on the crack during the in-situ observation process, and different test areas need to be refocused. The interrupted test SEM requires repeated disassembly of the test piece, which is a cumbersome and complicated process. In addition, the blade-like structural parts are large in size and cannot be placed in the SEM cavity for testing. The operation process of cellulose acetate film replication is complicated. The surface needs to be polished before replication. During replication, acetone needs to be repeatedly applied and a hair dryer needs to be used for auxiliary curing. After replication, a dust-free flat plate needs to be used for storage. Related research work has shown that the use of this process for replication will lead to a significant increase in the fatigue life of the specimen, affecting the test results. The operation of silicone rubber replication is simple, the curing time is short, there are no requirements for the shape and surface state of the component, and it is easy to store after curing. The crack replication method does not require disassembly of the test piece, which greatly simplifies the test process and avoids test errors caused by repeated disassembly of the test piece.
[0004] Patent application with publication number CN108375514A proposes an experimental method for obtaining the fatigue small crack conditions of metal plates by replicating with cellulose acetate film. Patent application with publication number CN112525735A discloses a replication method for detecting fatigue small crack conditions, which is optimized on the basis of the method disclosed in CN108375514A and improves the success rate of crack replication. It is true that the technology of using cellulose acetate film for crack replication has become mature, but the traditional method is cumbersome to operate and has low experimental efficiency. Summary of the invention
[0005] The main purpose of the present invention is to propose an experimental method for obtaining fatigue crack conditions of the leading edge of a blade with foreign object damage, aiming to solve the above technical problems.
[0006] To achieve the above object, the present invention proposes an experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage, comprising the following steps:
[0007] S1. Determine the dangerous position of the leading edge of the blade being tested;
[0008] S2, determining the stress value at the dangerous position of the leading edge of the measured blade;
[0009] S3, making a silicone rubber curing device;
[0010] S4. Grind the dangerous area of the leading edge of the blade being tested;
[0011] S5, performing an interrupted fatigue test, after stopping the machine at a certain number of cycles, installing the silicone rubber curing device made in step S3 at a dangerous position on the leading edge of the blade to be tested, injecting silicone rubber and then performing replication, obtaining replicated silicone rubbers at different numbers of cycles and numbering them according to the number of cycles;
[0012] S6. Observe the test results and take photos;
[0013] S7. Process the image data to obtain the overall morphology of the crack.
[0014] Preferably, in step S1, the method for determining the dangerous position of the leading edge of the measured blade is: using the finite element method to perform numerical simulation on the measured blade, extracting the modal stress calculation results under the first-order vibration mode, and delineating the high stress area of the leading edge; in the first calculation result, selecting a section of the highest stress point on the leading edge in each direction of the blade tip and the blade root, refining the grid size, and performing numerical simulation calculations again to obtain the precise coordinates of the high stress point on the leading edge, which is the dangerous point on the leading edge of the blade.
[0015] Preferably, in step S2, the method for determining the stress value at the dangerous position of the leading edge of the measured blade is: in the numerical simulation calculation results, the low stress gradient area of the blade body is selected as the strain gauge pasting position, and the simulated modal stress values of these positions are extracted; a conversion relationship between each strain gauge pasting point and the leading edge dangerous point is established, and the stress value at the leading edge dangerous point is calculated by detecting the stress value at the strain gauge.
[0016] Preferably, the silicone rubber curing device includes a main cavity for being installed on the blade basin side and the back side of the measured blade, and a sub-cavity for being installed on the arc part of the leading edge of the measured blade; a first chamber is arranged on the main cavity, and a second chamber is arranged on the sub-cavity; the first chamber of the two main cavities is connected with the second chamber of the sub-cavity to jointly constitute a silicone rubber containing chamber; an insert block is arranged on the sub-cavity, and a slot is arranged on the main cavity; a plurality of wedge-shaped holes are arranged on the sub-cavity, and wedge blocks are inserted in the wedge-shaped holes; in step S5, when the silicone rubber curing device is installed at the dangerous position of the leading edge of the measured blade, the insert block of the sub-cavity is inserted into the slot of the main cavity, and the wedge block is inserted into the wedge-shaped hole of the sub-cavity, the tip of the wedge block penetrates into the second chamber of the sub-cavity, and the tip of the wedge block is spaced apart from the arc surface of the leading edge of the measured blade.
[0017] Preferably, in step S3, when manufacturing the silicone rubber curing device, it is necessary to perform three-dimensional modeling on the two main cavities, including the following steps:
[0018] S301, determining a reference plane: taking a plane at the blade height where the maximum stress point of the leading edge of the blade is located as the reference plane, and the reference plane is parallel to the edge plate plane of the blade being measured;
[0019] S302, performing curve stretching: the reference plane intersects with the leading edge of the measured blade to obtain a blade basin side curve, a blade back side curve and an arc segment curve respectively; determining the center of the arc segment curve; stretching the blade basin side curve and the blade back side curve from the center of the circle toward the blade tip and the blade root respectively to obtain two curved surfaces respectively, and offsetting the two curved surfaces outward to form two initial geometric bodies, using the model of the measured blade as a tool, performing Boolean subtraction operations on the two initial geometric bodies respectively, that is, subtracting the part of the measured blade from the two initial geometric bodies to obtain two new geometric bodies;
[0020] S303, shell extraction: select two surfaces of two new geometric bodies that are in contact with the blade basin and the blade back, perform shell extraction on the two new geometric bodies, and obtain two cavity geometric bodies. Remove the end faces of the two cavity geometric bodies close to the leading edge to form a first cavity with two open sides. The two cavity geometric bodies are located on both sides of the blade, forming main cavity models for installation on the blade basin side and the blade back side respectively.
[0021] Preferably, in the step S3, when making the silicone rubber curing device, it is also necessary to perform three-dimensional modeling of the auxiliary cavity and the wedge block, including step S304, stretching the arc segment curve from the center of the circle toward the blade tip and the blade root to obtain an arc surface respectively, and biasing the arc surface outward to form a fan-shaped geometric body, using the model of the measured blade as a tool, performing a Boolean subtraction operation on the fan-shaped geometric body, and then performing a shell extraction operation, and opening a wedge-shaped hole to obtain a model of the auxiliary cavity; establishing a model of the wedge block according to the shape of the wedge-shaped hole; the wedge block is in the shape of an isosceles triangular prism.
[0022] Preferably, the specific operation of polishing the area where the dangerous position of the leading edge of the measured blade is located in step S4 is: before clamping the measured blade to the vibration table, polish the high stress area of the leading edge of the measured blade with sandpaper to avoid changing the structural dimensions of the leading edge during the polishing process, and after polishing until there are no scratches visible to the naked eye, use alcohol to clean the surface of the dangerous area of the leading edge; use sandpaper with a mesh size of 1500 or above for polishing.
[0023] Preferably, in step S5, the operation of interrupting the fatigue test is as follows: placing the blade to be tested on an electronically controlled vibration table, carrying out fatigue testing of the blade to be tested after applying a load, and stopping the machine after a certain number of cycles; combining two main cavities and one auxiliary cavity of the silicone rubber curing device and fixing them in the dangerous point area of the leading edge of the blade, firstly injecting silicone rubber into the first cavity of the two main cavities, and when the silicone rubber fills the first cavity of the main cavity, covering the wedge block with plastic wrap and inserting the auxiliary cavity in turn, and continuing to inject silicone rubber into the second cavity from the wedge hole where the wedge block has not been inserted, until it is completely filled, and inserting the last wedge block; after completing the injection of the replica silicone rubber, standing and waiting for the silicone rubber to cure, after the curing is completed, pulling out the wedge blocks in turn, peeling off the plastic wrap, dismantling the main cavity, and finally removing the cured silicone rubber from the auxiliary cavity and laying it flat, storing it and recording it by number, and completing one replication; continuing to apply load to the blade, repeating the replication operation, obtaining replica silicone rubber under different number of cycles and numbering it according to the number of cycles.
[0024] Preferably, in step S6, the method for observing the test results is: placing the flat cured replica silicone rubber under an optical microscope for observation, observing the sample from most to least cycles, until no cracks are observed on the replica silicone rubber sample; the method for taking pictures is: finding the end point of the crack from one side, selecting a microscope lens magnification that can clearly observe the crack, photographing the crack morphology in sequence at the same magnification until the entire crack is imaged, and numbering the images in the order in which they are photographed.
[0025] Preferably, the specific operation of processing the image data in step S7 is: measuring the crack length in the image, dividing the main crack extension path into small segments that are approximately straight lines, measuring each small crack segment separately, and summing them up to obtain the total crack length.
[0026] Due to the adoption of the above technical solution, the beneficial effects of the present invention are as follows:
[0027] (1) The present invention uses a silicone rubber curing device to replicate cracks. When replicating, only the dangerous position of the leading edge of the blade to be tested needs to be replicated. By observing the crack conditions on the replica silicone rubber under different cycle times, the fatigue crack conditions of the leading edge of the blade damaged by foreign objects can be obtained. The operation is simple and convenient, and it is also conducive to improving the experimental efficiency.
[0028] (2) The silicone rubber curing device used in the present invention, since the wedge block occupies the volume of the front edge arc segment, can form a plurality of wedge-shaped openings on the outer surface of the cured replica silicone rubber, so that the replica silicone rubber can be deformed from a V-shaped state to a nearly flat state when it is self-flattened, which is convenient for observing the test results and taking pictures.
[0029] (3) The silicone rubber curing device used in the present invention is easy and convenient to disassemble and can be used repeatedly. There is no need to disassemble the test piece during the experiment. When assembling, it is only necessary to insert the plug of the auxiliary cavity into the slot of the main cavity and insert the wedge block into the wedge hole of the auxiliary cavity. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0031] Figure 1 It is an assembly diagram of the blade to be tested and the silicone rubber curing device in the present invention;
[0032] Figure 2 A schematic diagram of constructing a reference plane on the blade being measured;
[0033] Figure 3 It is a structural schematic diagram of the main cavity in the present invention;
[0034] Figure 4 It is a schematic diagram of the structure of the auxiliary cavity in the present invention;
[0035] Figure 5 It is a schematic diagram of the structure of the wedge block in the present invention;
[0036] Figure 6 Comparison of the cured replica silicone rubber when it is flattened to form several wedge-shaped openings and non-wedge-shaped openings.
[0037] Explanation of the accompanying figures: 1. Measured blade; 2. Main cavity; 2a. First cavity; 2b. Slot; 3. Sub-cavity; 3a. Second cavity; 3b. Insert block; 3c. Wedge-shaped hole; 4. Wedge-shaped block; 4a. Handle; 5. Reference plane; 6. Edge plate plane; 7. Center of circle; 8. Blade basin side curve; 9. Blade back side curve; 10. Arc segment curve. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0040] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0041] As shown in the accompanying drawings, an experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage includes the following steps:
[0042] Step S1, determine the dangerous position of the leading edge of the measured blade 1: use the finite element method to perform numerical simulation on the measured blade 1, extract the modal stress calculation results under the first-order vibration mode, and define the high stress area of the leading edge; in the first calculation result, select a section of the highest stress point on the leading edge in each direction of the blade tip and the blade root, refine the grid size, and perform numerical simulation calculation again to obtain the precise coordinates of the high stress point on the leading edge, which is the dangerous point on the leading edge of the blade
[0043] Step S2, determining the stress value at the dangerous position of the leading edge of the measured blade 1: in the numerical simulation calculation results, select the low stress gradient area of the blade body as the strain gauge pasting position, and extract the simulated modal stress values of these positions; establish a conversion relationship between each strain gauge pasting point and the leading edge dangerous point, and calculate the stress value at the leading edge dangerous point by detecting the stress value at the strain gauge.
[0044] Step S3, making a silicone rubber curing device: the silicone rubber curing device includes a main cavity 2 for being installed on the blade basin side and the back side of the measured blade 1, and a sub-cavity 3 for being installed on the arc portion of the leading edge of the measured blade 1; a first cavity 2a is arranged on the main cavity 2, and a second cavity 3a is arranged on the sub-cavity 3; the first cavity 2a of the two main cavities 2 is connected with the second cavity 3a of the sub-cavity 3 to form a silicone rubber containing cavity; an insert block 3b is arranged on the sub-cavity 3, and a slot 2 is arranged on the main cavity 2; a plurality of wedge-shaped holes 3c are arranged on the sub-cavity 3, and wedge blocks 4 are inserted into the wedge-shaped holes 3c.
[0045] When manufacturing the silicone rubber curing device, it is necessary to perform three-dimensional modeling of the two main cavities 2, including the following steps:
[0046] Step S301 , determining a reference plane 5 : taking a plane at the blade height where the maximum stress point of the leading edge of the blade is located as the reference plane 5 , and the reference plane 5 is parallel to the edge plate plane 6 of the blade 1 to be measured.
[0047] Step S302, perform curve stretching: the reference plane 5 intersects with the leading edge of the measured blade 1 to obtain a blade basin side curve 8, a blade back side curve 9 and an arc segment curve 10; determine the center 7 of the arc segment curve 10; stretch the blade basin side curve 8 and the blade back side curve 9 toward the blade tip and the blade root with the center 7 to obtain two curved surfaces, and offset the two curved surfaces outward to form two initial geometric bodies, use the model of the measured blade 1 as a tool, perform Boolean subtraction operations on the two initial geometric bodies, that is, subtract the part of the measured blade 1 from the two initial geometric bodies to obtain two new geometric bodies, one of which is completely fitted with the blade basin, and the other is completely fitted with the blade back.
[0048] Step S303, shell extraction: select two surfaces of two new geometric bodies that are in contact with the blade basin and the blade back, perform shell extraction on the two new geometric bodies, the shell thickness is 2mm, and two cavity geometric bodies are obtained. The end faces of the two cavity geometric bodies close to the leading edge are removed to form a first chamber 2a with two open sides, and a 5mm×5mm×1mm slot 2b is opened on the side of the cavity geometric body close to the leading edge. The two cavity geometric bodies are located on both sides of the blade, respectively, to form a main cavity 2 model for installation on the blade basin side and the blade back side.
[0049] It is also necessary to perform three-dimensional modeling on the auxiliary cavity 3 and the wedge block 4, so step S3 also includes:
[0050] Step S304, stretch the arc segment curve 10 in the direction of the blade tip and the blade root with the center of the circle 7 to obtain an arc surface respectively, and offset the arc surface outward to form a fan-shaped geometric body, use the model of the measured blade 1 as a tool, perform a Boolean subtraction operation on the fan-shaped geometric body, and then perform a shell extraction operation, open five wedge-shaped holes 3c, and set plug blocks 3b on both sides to obtain a model of the sub-cavity 3; establish a model of the wedge block 4 according to the shape of the wedge-shaped hole 3c; the wedge block 4 is in the shape of an isosceles triangular prism.
[0051] Through the above steps, a three-dimensional model of the main cavity 2, the auxiliary cavity 3, and the wedge block 4 is obtained, and the main cavity 2, the auxiliary cavity 3, and the wedge block 4 are processed according to the three-dimensional model. In order to facilitate the insertion and removal of the wedge block 4, a handle 4a is provided on the wedge block 4.
[0052] Step S4, grinding the dangerous area of the leading edge of the measured blade 1: before clamping the measured blade 1 to the vibration table, use sandpaper to grind the high stress area of the leading edge of the measured blade 1 to avoid changing the structural dimensions of the leading edge during the grinding process. After grinding until there are no visible scratches to the naked eye, use alcohol to clean the surface of the dangerous area of the leading edge; use sandpaper with a mesh size of 1500 or above for grinding.
[0053] Step S5, perform an interrupted fatigue test, install the silicone rubber curing device produced in step S3 at the dangerous position of the leading edge of the measured blade 1 after stopping the machine at certain number of cycles, inject silicone rubber and perform replication to obtain the replicated silicone rubber at different number of cycles and number them according to the number of cycles: when the silicone rubber curing device is installed at the dangerous position of the leading edge of the measured blade 1, the plug 3b of the auxiliary cavity 3 is inserted into the slot 2b of the main cavity 2, and the wedge block 4 is inserted into the wedge-shaped hole 3c of the auxiliary cavity 3, the tip of the wedge block 4 penetrates into the second chamber 3a of the auxiliary cavity 3, and the tip of the wedge block 4 is spaced apart from the arc surface of the leading edge of the measured blade 1. Specifically, the operation of the interrupted fatigue test is as follows: the blade 1 to be tested is placed on an electronically controlled vibration table, and after applying a load, a fatigue test of the blade 1 to be tested is carried out, and the machine is stopped after a certain number of cycles; two main cavities 2 and one auxiliary cavity 3 of the silicone rubber curing device are combined and fixed in the dangerous point area of the leading edge of the blade, and silicone rubber is first injected into the first cavity 2a of the two main cavities 2. When the silicone rubber fills the first cavity 2a of the main cavity 2, the cling film is covered on the wedge block 4, and the auxiliary cavity 3 is inserted in turn, and the wedge block 4 is not inserted. Continue to inject silicone rubber into the second chamber 3a through the wedge-shaped hole 3c until it is completely filled, and insert the last wedge-shaped block 4; after completing the injection of the replica silicone rubber, wait for the silicone rubber to solidify. After the solidification is completed, pull out the wedge-shaped blocks 4 in turn, peel off the plastic wrap, remove the main cavity 2, and finally remove the solidified silicone rubber from the auxiliary cavity 3 and lay it flat, store it, and record it by number, completing one replication; continue to apply load to the blade 1, repeat the replication operation, obtain the replica silicone rubber under different cycle numbers and number them according to the cycle number.
[0054] Combination Figure 6 As shown, since the wedge block 4 occupies the volume of the front arc segment, the cured complex silicone rubber can be deformed from a V-shaped state to an approximately flat state 16. In comparison, the cured silicone rubber without the wedge block 4 will be squeezed at the bottom and deformed on the surface to produce wrinkles after being laid flat due to the difference in length of the inner and outer arc segments. The planar state silicone rubber cured after the wedge block 4 is used will greatly simplify the observation of cracks.
[0055] Step S6, observe the test results and take photos: The method of observing the test results is: place the flat cured replica silicone rubber under an optical microscope for observation, and observe the sample from the most to the least number of cycles until no cracks are observed on the replica silicone rubber sample. The method of taking photos is: find the end point of the crack from one side, select a microscope lens magnification that can clearly observe the crack, and take photos of the crack morphology in sequence at the same magnification until the entire crack is captured, and number the images according to the order in which they are taken.
[0056] Step S7: Process the image data to obtain the overall crack morphology. Measure the crack length in the image, divide the main crack extension path into small segments that are approximately straight lines, measure each small crack segment separately, and sum them up to obtain the total crack length.
[0057] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. An experimental method for obtaining fatigue crack conditions at the leading edge of a blade due to foreign object damage, characterized in that: The steps include: S1. determining the dangerous position of the leading edge of the blade (1) to be tested; S2, determining the stress value at the dangerous position of the leading edge of the blade (1) under test; S3, making a silicone rubber curing device; S4, grinding the area where the dangerous position of the leading edge of the blade (1) to be tested is located; S5, performing an interrupted fatigue test, after stopping the machine at a certain number of cycles, installing the silicone rubber curing device produced in step S3 at a dangerous position on the leading edge of the blade (1) to be tested, injecting silicone rubber and then performing replication, obtaining replicated silicone rubbers at different numbers of cycles and numbering them according to the number of cycles; S6. Observe the test results and take photos; S7. Process the image data to obtain the overall morphology of the crack.
2. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage according to claim 1, characterized in that: In step S1, the method for determining the dangerous position of the leading edge of the measured blade (1) is as follows: using the finite element method to perform numerical simulation on the measured blade (1), extracting the modal stress calculation results under the first-order vibration mode, and defining the high stress area of the leading edge; in the first calculation result, selecting a region in each direction of the blade tip and the blade root from the highest stress point of the leading edge, refining the grid size, and performing numerical simulation calculation again to obtain the precise coordinates of the high stress point of the leading edge, which is the dangerous point of the leading edge of the blade.
3. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage as claimed in claim 2, characterized in that: In step S2, the method for determining the stress value at the dangerous position of the leading edge of the measured blade (1) is as follows: in the numerical simulation calculation results, the low stress gradient area of the blade body is selected as the strain gauge pasting position, and the simulated modal stress values of these positions are extracted; the conversion relationship between each strain gauge pasting point and the leading edge dangerous point is established, and the stress value at the leading edge dangerous point is calculated by detecting the stress value at the strain gauge.
4. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage according to claim 1, characterized in that: The silicone rubber curing device comprises a main cavity (2) for being installed on the blade base side and the blade back side of the measured blade (1), and a secondary cavity (3) for being installed on the arc portion of the leading edge of the measured blade (1); a first cavity (2a) is arranged on the main cavity (2), and a second cavity (3a) is arranged on the secondary cavity (3); the first cavity (2a) of the two main cavities (2) and the second cavity (3a) of the secondary cavity (3) are connected to form a silicone rubber containing cavity; an insert block (3b) is arranged on the secondary cavity (3), and a slot is arranged on the main cavity (2). (2); a plurality of wedge-shaped holes (3c) are provided on the auxiliary cavity (3), and wedge-shaped blocks (4) are inserted into the wedge-shaped holes (3c); in step S5, when the silicone rubber curing device is installed at the dangerous position of the leading edge of the measured blade (1), the insert block (3b) of the auxiliary cavity (3) is inserted into the slot (2b) of the main cavity (2), and the wedge-shaped block (4) is inserted into the wedge-shaped hole (3c) of the auxiliary cavity (3), the tip of the wedge-shaped block (4) penetrates into the second chamber (3a) of the auxiliary cavity (3), and the tip of the wedge-shaped block (4) is spaced from the arc surface of the leading edge of the measured blade (1).
5. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage as claimed in claim 4, characterized in that: In step S3, when manufacturing the silicone rubber curing device, it is necessary to perform three-dimensional modeling on the two main cavities (2), including the following steps: S301, determining a reference plane (5): taking a plane at the blade height where the maximum stress point of the blade leading edge is located as the reference plane (5), and the reference plane (5) is parallel to the edge plate plane (6) of the blade (1) to be measured; S302, performing curve stretching: the reference plane (5) intersects with the leading edge of the measured blade (1) to obtain a blade basin side curve (8), a blade back side curve (9) and an arc segment curve (10); determining the center (7) of the arc segment curve (10); stretching the blade basin side curve (8) and the blade back side curve (9) from the center (7) toward the blade tip and the blade root to obtain two curved surfaces, and offsetting the two curved surfaces outward to form two initial geometric bodies, using the model of the measured blade (1) as a tool, performing a Boolean subtraction operation on the two initial geometric bodies, that is, subtracting the part of the measured blade (1) from the two initial geometric bodies to obtain two new geometric bodies; S303, shell extraction processing: select two surfaces of two new geometric bodies that are in contact with the blade basin and the blade back, perform shell extraction operations on the two new geometric bodies, and obtain two cavity geometric bodies. Remove the end faces of the two cavity geometric bodies close to the leading edge to form a first cavity (2a) with two open sides. The two cavity geometric bodies are respectively located on both sides of the blade, forming main cavity (2) models for installation on the blade basin side and the blade back side.
6. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage as claimed in claim 5, characterized in that: In the step S3, when manufacturing the silicone rubber curing device, it is also necessary to perform three-dimensional modeling on the auxiliary cavity (3) and the wedge block (4), including step S304, stretching the arc segment curve (10) from the center of the circle (7) toward the blade tip and the blade root to obtain an arc surface respectively, and biasing the arc surface outward to form a fan-shaped geometric body, using the model of the measured blade (1) as a tool, performing a Boolean subtraction operation on the fan-shaped geometric body, and then performing a shell extraction operation, and opening a wedge-shaped hole (3c) to obtain a model of the auxiliary cavity (3); establishing a model of the wedge block (4) according to the shape of the wedge-shaped hole (3c); the wedge block (4) is in the shape of an isosceles triangular prism.
7. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage according to claim 1, characterized in that: The specific operation of step S4 of grinding the area where the dangerous position of the leading edge of the measured blade (1) is located is as follows: before the measured blade (1) is clamped on the vibration table, the high stress area of the leading edge of the measured blade (1) is ground with sandpaper to avoid changing the structural dimensions of the leading edge during the grinding process; after grinding until there are no scratches visible to the naked eye, the surface of the dangerous area of the leading edge is cleaned with alcohol; sandpaper with a mesh size of 1500 or above is used for grinding.
8. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage as claimed in claim 4, characterized in that: In step S5, the operation of performing the interrupted fatigue test is as follows: placing the blade (1) to be tested on an electronically controlled vibration table, applying a load and then performing a fatigue test on the blade (1), and stopping the machine after a certain number of cycles; combining and fixing two main cavities (2) and one auxiliary cavity (3) of a silicone rubber curing device in a dangerous area at the leading edge of the blade, firstly injecting silicone rubber into the first cavity (2a) of the two main cavities (2), and when the silicone rubber fills the first cavity (2a) of the main cavity (2), covering the wedge block (4) with a plastic wrap and inserting the auxiliary cavity (3) in turn, and then inserting the silicone rubber into the auxiliary cavity (3) without inserting the silicone rubber into the wedge block (4). The wedge-shaped hole (3c) of the wedge-shaped block (4) continues to inject silicone rubber into the second chamber (3a) until it is completely filled, and then the last wedge-shaped block (4) is inserted; after the injection of the replica silicone rubber is completed, the silicone rubber is left to stand and solidify, and after the solidification is completed, the wedge-shaped blocks (4) are pulled out in turn, the plastic wrap is peeled off, the main chamber (2) is removed, and finally the solidified silicone rubber is taken out from the auxiliary chamber (3) and laid flat, stored and numbered, and one replication is completed; the load is continued to be applied to the blade (1), and the replication operation is repeated to obtain replica silicone rubbers under different cycle numbers and number them according to the cycle number.
9. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage as claimed in claim 1, characterized in that: In step S6, the operation method of observing the test results is: placing the flat cured replica silicone rubber under an optical microscope for observation, and observing the sample from the most to the least number of cycles until no cracks are observed on the replica silicone rubber sample; The method of taking pictures is as follows: find the end point of the crack from one side, select a microscope lens magnification that can clearly observe the crack, and photograph the crack morphology in sequence at the same magnification until the entire crack is imaged, and number the images in the order in which they were taken.
10. The experimental method for obtaining fatigue crack conditions of the leading edge of a blade due to foreign object damage according to claim 9, characterized in that: The specific operation of processing the image data in step S7 is: measuring the crack length in the image, dividing the main crack extension path into small segments that are approximately straight lines, measuring each small crack segment separately, and summing them up to obtain the total crack length.
Citation Information
Cited By
Detection equipment for blower production
CN119666424A
A testing equipment for hair dryer production
CN119666424B