High-molybdenum-equivalent metastable beta titanium alloy workpiece, preparation method and application of high-molybdenum-equivalent metastable beta titanium alloy workpiece

Through plasma rotary electrode method and thermal isostatic pressure and solid solution aging treatment, high molybdenum equivalent metastable β titanium alloy parts were prepared, which solved the problem of difficult to take into account both high strength and high plastic toughness in the existing technology, and realized titanium The excellent mechanical properties of the alloy are suitable for aerospace.

CN118989324APending Publication Date: 2024-11-22SINO EURO MATERIALS TECH OF XIAN CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411091089.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to take into account high strength and high plastic toughness in high molybdenum equivalent metastable β-titanium alloys, resulting in limited application under extreme working conditions.

Method used

The titanium alloy powder was prepared by plasma rotary electrode method. After thermal isostatic pressure and solid solution aging treatment, the tensile strength ≥1300MPa, yield strength ≥1200MPa, elongation ≥10%, impact toughness ≥25J·cm-2 was prepared. Molybdenum equivalent metastable β-titanium alloy parts.

Benefits of technology

It has achieved a balance of strong-plastic-toughness in titanium alloys, breaking through the limitations of sacrificing plastic toughness in traditional processes due to the pursuit of high strength, and providing better material options for aerospace and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989324A_ABST
    Figure CN118989324A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of non-ferrous metal processing, and particularly discloses a metastable beta titanium alloy workpiece with high molybdenum equivalent and a preparation method and application thereof.The preparation method comprises the steps that (1) titanium alloy powder is prepared and screened, the titanium alloy powder with the particle size being 53-150 microns and the oxygen content being 600-1200 ppm is obtained, the sphericity degree of the titanium alloy powder is required to be larger than or equal to 90%, and the hollow proportion of the titanium alloy powder is required to be smaller than or equal to 0.1%; 2) carrying out hot isostatic pressing treatment on the screened titanium alloy powder, wherein the hot isostatic pressing treatment comprises the operations of cleaning and drying a prefabricated sheath, vacuumizing and sealing, heating and boosting and the like to obtain an intermediate; and (3) the intermediate is subjected to two-phase region solid solution and aging treatment, and a target workpiece is obtained. According to the preparation method, a part with a micron-sized uniform structure and balanced strength-plasticity-toughness can be obtained, near-net forming of a complex structure is achieved, the material utilization rate is increased, the prepared metastable beta titanium alloy structural part with the high molybdenum equivalent can be used for novel aerospace vehicles, and it is guaranteed that the material preparation process is feasible and reliable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nonferrous metal processing, and in particular, relates to a high-molybdenum equivalent metastable β-titanium alloy product, a preparation method and an application thereof. Background Art

[0002] In today's booming field of materials science, titanium alloys have become an indispensable key material in many advanced engineering applications due to their excellent comprehensive performance. According to the way of classifying titanium alloys by molybdenum equivalent, high molybdenum equivalent is generally reflected in the "α+β" two-phase titanium alloy containing Mo, V, and Cr. This type of alloy has strong solid solution strengthening and second phase dispersion strengthening effects, so it has excellent high-temperature creep performance, durability and damage tolerance performance, which can greatly extend the service life and service cycle of aircraft engine structural parts. For example, the Ti45551 two-phase titanium alloy, which is regarded as a typical representative, has a molybdenum equivalent of about 18 and a β phase transformation temperature of about 795℃.

[0003] In addition, when the content of β-stable elements in titanium alloy exceeds 17%, it will be defined as a metastable β-titanium alloy. This type of titanium alloy always firmly maintains the unique characteristics of the "α+β" two-phase structure in a balanced state. After proper heat treatment, this type of titanium alloy has great potential to achieve extremely high room temperature strength while also showing relatively good plasticity and toughness.

[0004] Because of its outstanding performance characteristics, high molybdenum equivalent metastable β titanium alloy has shown great application potential in the aerospace field, especially in the manufacture of key load-bearing structural parts such as aircraft landing gear, wings and engine pylons. However, in terms of the current actual production situation, the manufacture of high molybdenum equivalent metastable β titanium alloy parts still relies heavily on traditional process methods, such as casting, forging and rolling. For example, taking the beam parts of a certain type of aircraft as an example, it uses high molybdenum equivalent metastable β titanium alloy forgings and undergoes two-phase solid solution aging treatment. Although a certain degree of optimization has been achieved in terms of performance, the actual data is not ideal. Specifically, the tensile strength is only in the range of 1150MPa to 1300MPa, the elongation is 6% to 8%, and the impact toughness is 20J•cm -2 ~28J•cm -2 In the range of 2000~2000mm, the tensile strength of a large-sized high-molybdenum equivalent metastable β titanium alloy after two-phase forging was increased to 1300MPa~1390MPa, but the elongation was very low, only 3%~6%, and the impact toughness was only 20J•cm -2 ~26J•cm -2 between.

[0005] In summary, the existing processes often expose significant shortcomings in terms of plasticity and toughness in the process of preparing ultra-high strength titanium alloys. This defect not only seriously restricts its wide application under more extreme and harsh working conditions, but also poses a challenge to the technological development in related fields. In order to break through this dilemma, it is urgent to develop an innovative preparation method that aims to perfectly match and achieve the perfect combination of high strength and high plasticity and toughness, thereby bringing breakthrough progress to the field of non-ferrous metal processing technology and meeting the market's growing and urgent demand for high-performance materials.

[0006] In view of this, this invention is proposed. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a high molybdenum equivalent metastable β titanium alloy product, a preparation method and its application, which are mainly used to solve the thorny problem of the difficulty in perfectly combining high strength with high plasticity and toughness in the traditional titanium alloy preparation process. The titanium alloy prepared by the process of the present invention not only achieves the balance of strength-plasticity-toughness, but also effectively solves the key problem of insufficient plasticity and toughness once the strength of the titanium alloy exceeds 1300MPa.

[0008] The purpose of the present invention is to be solved by the following technical solutions: In a first aspect, the present invention provides a method for preparing a high molybdenum equivalent metastable β titanium alloy product, comprising the following steps: Step 1: First, titanium alloy powder is prepared by a plasma rotating electrode method and sieved to obtain titanium alloy powder of a set particle size; Step 2: then subjecting the titanium alloy powder obtained in step 1 to hot isostatic pressing to obtain a titanium alloy intermediate; Step 3: Finally, the titanium alloy intermediate obtained in step 2 is subjected to a solid solution aging treatment to obtain a high molybdenum equivalent metastable β titanium alloy product.

[0009] Furthermore, in step one, the raw material used to prepare the titanium alloy powder is Ti45551 titanium alloy, and the chemical composition of the Ti45551 titanium alloy, measured in mass percentage, includes: Al: 3.9wt%~4.5wt%, Mo: 4.8wt%~5.5wt%, V: 4.9wt%~5.2wt%, Cr: 5.0wt%~5.8wt%, O: ≤0.12wt%, H: ≤0.005wt%, C: ≤0.01wt%, N: ≤0.01wt%, Fe: ≤0.05wt%, and the rest are Ti and unavoidable impurities.

[0010] Furthermore, in step one, the particle size range of the titanium alloy powder after screening is 53μm to 150μm, and the oxygen content of the titanium alloy powder is controlled between 600ppm and 1200ppm. At the same time, the sphericity of the titanium alloy powder is required to be greater than or equal to 90%, and the hollow ratio is less than or equal to 0.1%.

[0011] Further, in step 2, the hot isostatic pressing treatment includes the following operation process: 1) First, the prefabricated package is cleaned and dried, and after drying, the screened titanium alloy powder is placed in the package, and is compacted by means of a heating and vibration device; 2) Then, the package is evacuated in the temperature range of 350°C to 500°C until the vacuum degree is less than 1×10 -4 Pa, and continue for 4 hours to 10 hours, and then perform electron beam sealing welding on the sheath to remove residual gas and moisture in the titanium alloy powder; 3) Finally, the obtained sealing and welding sheath is heated to 720°C to 780°C and the pressure is increased to 120MPa to 180MPa under the conditions of synchronous temperature and pressure increase, and the temperature and pressure are maintained for 3h to 4h. After cooling to room temperature in the furnace, the sheath is removed to obtain a titanium alloy intermediate.

[0012] Furthermore, in step 1), the prefabricated sheath is cleaned with an acetone solution and dried by heating.

[0013] Furthermore, in step three, the solution aging treatment includes performing a solution treatment in a two-phase region and then performing an aging treatment.

[0014] Furthermore, in the step three, the solution treatment temperature is 730°C to 780°C, and the solution treatment time is 1h to 4h; the aging treatment temperature is 510°C to 580°C, and the aging treatment time is 4h to 8h, and after the solution treatment and aging treatment, the steel is air-cooled to room temperature.

[0015] In a second aspect, the present invention provides a high molybdenum equivalent metastable β-titanium alloy product, wherein the high molybdenum equivalent metastable β-titanium alloy product is prepared by the preparation method described above.

[0016] Furthermore, the mechanical properties of the high molybdenum equivalent metastable β titanium alloy product are as follows: tensile strength ≥ 1300MPa, yield strength ≥ 1200MPa, elongation ≥ 10%, impact toughness ≥ 25J•cm -2 .

[0017] In a third aspect, the present invention provides a high molybdenum equivalent metastable β-titanium alloy product prepared by the above-mentioned preparation method, or the use of the high molybdenum equivalent metastable β-titanium alloy product described above in aircraft load-bearing parts.

[0018] Compared with the prior art, the present invention has the following beneficial effects: The preparation method provided by the present invention has a process route of: powder making and screening → hot isostatic pressing → solution aging treatment. In the specific operation, by strictly controlling the particle size, oxygen content, sphericity and hollow ratio of the titanium alloy powder, and accurately setting the process conditions of hot isostatic pressing and solution aging treatment, the stability and consistency of the performance of the titanium alloy parts are ensured. After actual verification, the titanium alloy parts prepared by the present invention show excellent performance: tensile strength ≥1300MPa, yield strength ≥1200MPa, elongation ≥10%, impact toughness ≥25J•cm -2 This achievement effectively solves the problem of high strength and high plasticity and toughness. It breaks through the limitations of traditional processes and no longer sacrifices plasticity and toughness in pursuit of high strength, providing a better material option for the wide application of high molybdenum equivalent metastable β titanium alloys in cutting-edge fields such as aerospace. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 It is a flow chart of the method for preparing a high molybdenum equivalent metastable β titanium alloy product of the present invention; Figure 2 This is the microstructure of the titanium alloy product prepared in Example 1 of the present invention. Figure 1 ; Figure 3 This is the microstructure of the titanium alloy product prepared in Example 1 of the present invention. Figure 2 . DETAILED DESCRIPTION

[0022] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples consistent with some aspects of the present invention as detailed in the appended claims.

[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.

[0024] See also Figure 1 The present invention provides a method for preparing a high molybdenum equivalent metastable β titanium alloy product, which specifically comprises the following steps: Step 1: Use the ultra-high speed plasma rotating electrode method (SS-PREP®) to prepare titanium alloy powder, and then screen it to obtain titanium alloy powder of a set particle size. Among them, the particle size range of the titanium alloy powder after screening is 53μm to 150μm, and the oxygen content of the titanium alloy powder is controlled between 600ppm and 1200ppm. At the same time, the sphericity of the titanium alloy powder is required to be greater than or equal to 90%, and the hollow ratio is less than or equal to 0.1%.

[0025] Among them, the raw material used for preparing the titanium alloy powder is Ti45551 titanium alloy, and the chemical composition of the Ti45551 titanium alloy is measured by mass percentage, including: Al: 3.9wt%~4.5wt%, Mo: 4.8wt%~5.5wt%, V: 4.9wt%~5.2wt%, Cr: 5.0wt%~5.8wt%, O: ≤0.12wt%, H: ≤0.005wt%, C: ≤0.01wt%, N: ≤0.01wt%, Fe: ≤0.05wt%, and the rest is Ti and unavoidable impurities. In addition, the molybdenum equivalent of the Ti45551 titanium alloy raw material used in this application is as high as 18, and the β phase transformation temperature is about 795°C.

[0026] Step 2: Perform hot isostatic pressing on the titanium alloy powder obtained above to obtain a titanium alloy intermediate. The operation process of hot isostatic pressing is as follows: first, clean the prefabricated package with acetone solution and heat and dry it. After drying, place the screened titanium alloy powder into the package and make it dense with the help of heating and vibration equipment; second, evacuate the package in the temperature range of 350℃ to 500℃ until the vacuum degree is less than 1×10 -4 Pa, and continue for 4h to 10h, followed by electron beam sealing treatment to remove residual gas and moisture in the titanium alloy powder; finally, the sealing package is heated to 720℃~780℃ and the pressure is increased to 120MPa~180MPa under the conditions of synchronous temperature and pressure increase, and the temperature and pressure are maintained for 3h to 4h. After cooling to room temperature with the furnace, the package is removed to obtain a titanium alloy intermediate.

[0027] Step 3: subjecting the obtained titanium alloy intermediate to a solution aging treatment, including a solution treatment in a two-phase region, followed by an aging treatment, to obtain a high molybdenum equivalent metastable β titanium alloy product.

[0028] Among them, the system of solution aging treatment is as follows: the solution treatment temperature is 730℃~780℃, and the solution treatment time is 1h~4h; the aging treatment temperature is 510℃~580℃, and the aging treatment time is 4h~8h, and after the solution treatment and aging treatment, the steel is air cooled to room temperature (AC).

[0029] In order to further verify the efficacy of the present invention, the inventors conducted the following experiments: Example 1

[0030] This embodiment aims to prepare a titanium alloy part with a diameter of 150 mm. The specific preparation process is as follows: 1) Ti45551 titanium alloy rods with a diameter of 79 mm were selected, and titanium alloy powder was prepared by ultra-high speed plasma rotating electrode method (SS-PREP®). Then, powder with a particle size in the range of 53 μm to 150 μm was obtained by sieving, while ensuring that the oxygen content was controlled at 900 ± 20 ppm, the sphericity was greater than or equal to 90%, and the hollow ratio was less than or equal to 0.1%.

[0031] 2) First, the titanium alloy powder sieved in step 1) is filled into a 20# steel ladle that has been cleaned with acetone and heated and dried, and then compacted by a heating and vibration device; then, vacuum is continuously drawn at 450°C until the vacuum degree is less than 1×10 -4 Pa, and continued for 6 hours, followed by electron beam sealing; finally, the sealing package was heated to 780°C under the conditions of synchronous temperature and pressure increase, and a pressure of 120MPa was applied at the same time, and the temperature and pressure were maintained for 3 hours. After cooling to room temperature with the furnace, the package was removed to obtain a titanium alloy intermediate with a diameter of 150mm.

[0032] 3) For the titanium alloy intermediate obtained in step 2), a solution treatment at 730℃ / 4h / AC and an aging treatment at 510℃ / 8h / AC were performed in sequence, and finally a titanium alloy part with a diameter of 150mm was successfully produced. The internal microstructure of the titanium alloy part is shown in FIG. Figure 2 , 3 As shown, it can be found through observation that its internal organization is evenly distributed and presents the characteristics of high densification.

[0033] The present invention also conducted mechanical tests on the titanium alloy parts prepared in this embodiment. The test results show that the titanium alloy parts treated by the process of the present invention have excellent mechanical properties, and the specific properties are as follows: the average tensile strength is 1339MPa, the average yield strength is 1252MPa, the average elongation is 10.5%, and the average impact toughness is 26.6J•cm -2 , showing good comprehensive matching characteristics of strength, plasticity and toughness. Example 2

[0034] This embodiment aims to prepare a titanium alloy part with a diameter of 100 mm. The specific preparation process is as follows: 1) Ti45551 titanium alloy rods with a diameter of 79 mm were selected, and the ultra-high speed plasma rotating electrode method (SS-PREP®) was used to prepare titanium alloy powder. Then, the powder with a particle size in the range of 53 μm to 150 μm was obtained by sieving, while ensuring that the oxygen content was controlled at 1100 ± 20 ppm, the sphericity was greater than or equal to 90%, and the hollow ratio was less than or equal to 0.1%.

[0035] 2) First, the titanium alloy powder sieved in step 1) is filled into a 20# steel ladle that has been cleaned with acetone and heated and dried, and then compacted with a heating and vibration device; then, vacuum is continuously drawn at 500°C until the vacuum degree is less than 1×10 -4 Pa, and continued for 4 hours, followed by electron beam sealing; finally, the sealing package was heated to 750°C under the conditions of synchronous temperature and pressure increase, and a pressure of 150MPa was applied at the same time, and the temperature and pressure were maintained for 3.5 hours. After cooling to room temperature with the furnace, the package was removed to obtain a titanium alloy intermediate with a diameter of 100mm.

[0036] 3) For the titanium alloy intermediate obtained in step 2), a solution treatment at 750°C / 2h / AC and an aging treatment at 550°C / 6h / AC were performed in sequence, and finally a titanium alloy part with a diameter of 100mm was successfully produced.

[0037] The present invention also conducted mechanical tests on the titanium alloy parts prepared in this embodiment. The test results show that the titanium alloy parts treated by the process of the present invention have excellent mechanical properties, and the specific properties are as follows: the average tensile strength is 1316MPa, the average yield strength is 1200MPa, the average elongation is 12.2%, and the average impact toughness is 25.1J•cm -2 , showing good comprehensive matching characteristics of strength, plasticity and toughness. Example 3

[0038] This embodiment aims to prepare a titanium alloy part with a diameter of 60 mm. The specific preparation process is as follows: 1) Ti45551 titanium alloy rods with a diameter of 79 mm were selected, and titanium alloy powder was prepared by ultra-high speed plasma rotating electrode method (SS-PREP®). Then, powder with a particle size in the range of 53 μm to 150 μm was obtained by sieving, while ensuring that the oxygen content was controlled at 700 ± 20 ppm, the sphericity was greater than or equal to 90%, and the hollow ratio was less than or equal to 0.1%.

[0039] 2) First, the titanium alloy powder sieved in step 1) is filled into a 20# steel ladle that has been cleaned with acetone and heated and dried, and then compacted by a heating and vibration device; then, vacuum is continuously drawn at 350°C until the vacuum degree is less than 1×10 -4 Pa, and continue for 10 hours, followed by electron beam sealing; finally, the sealing package is heated to 720°C under the conditions of synchronous temperature and pressure increase, and a pressure of 180MPa is applied at the same time, and the temperature and pressure are maintained for 4 hours. After cooling to room temperature with the furnace, the package is removed to obtain a titanium alloy intermediate with a diameter of 60mm.

[0040] 3) For the titanium alloy intermediate obtained in step 2), a solution treatment at 780°C / 1h / AC and an aging treatment at 580°C / 4h / AC were performed in sequence, and finally a titanium alloy part with a diameter of 150mm was successfully produced.

[0041] The present invention also conducted mechanical tests on the titanium alloy parts prepared in this embodiment. The test results show that the titanium alloy parts treated by the process of the present invention have excellent mechanical properties, and the specific properties are as follows: the average tensile strength is 1327MPa, the average yield strength is 1201MPa, the average elongation is 11.2%, and the average impact toughness is 28.0J•cm -2 , showing good comprehensive matching characteristics of strength, plasticity and toughness.

[0042] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0043] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a high molybdenum equivalent metastable β titanium alloy product, characterized in that: The following steps are involved: Step 1: First, titanium alloy powder is prepared by a plasma rotating electrode method and sieved to obtain titanium alloy powder of a set particle size; Step 2: then subjecting the titanium alloy powder obtained in step 1 to hot isostatic pressing to obtain a titanium alloy intermediate; Step 3: Finally, the titanium alloy intermediate obtained in step 2 is subjected to a solid solution aging treatment to obtain a high molybdenum equivalent metastable β titanium alloy product.

2. The method for preparing a high molybdenum equivalent metastable β titanium alloy product according to claim 1, characterized in that: In step one, the raw material used to prepare the titanium alloy powder is Ti45551 titanium alloy. The chemical composition of the Ti45551 titanium alloy, measured in mass percentage, includes: Al: 3.9wt%~4.5wt%, Mo: 4.8wt%~5.5wt%, V: 4.9wt%~5.2wt%, Cr: 5.0wt%~5.8wt%, O: ≤0.12wt%, H: ≤0.005wt%, C: ≤0.01wt%, N: ≤0.01wt%, Fe: ≤0.05wt%, and the rest are Ti and unavoidable impurities.

3. The method for preparing a high molybdenum equivalent metastable β titanium alloy product according to claim 1, characterized in that: In step one, the particle size range of the titanium alloy powder after screening is 53μm to 150μm, and the oxygen content of the titanium alloy powder is controlled between 600ppm and 1200ppm. At the same time, the sphericity of the titanium alloy powder is required to be greater than or equal to 90%, and the hollow ratio is less than or equal to 0.1%.

4. The method for preparing a high molybdenum equivalent metastable β titanium alloy product according to claim 1, characterized in that: In step 2, the hot isostatic pressing process includes the following operation flow: 1) First, the prefabricated package is cleaned and dried, and after drying, the screened titanium alloy powder is placed in the package, and is compacted by means of a heating and vibration device; 2) Then, the package is evacuated in the temperature range of 350°C to 500°C until the vacuum degree is less than 1×10 -4 Pa, and continue for 4 hours to 10 hours, and then perform electron beam sealing welding on the sheath to remove residual gas and moisture in the titanium alloy powder; 3) Finally, the obtained sealing and welding sheath is heated to 720°C to 780°C and the pressure is increased to 120MPa to 180MPa under the conditions of synchronous temperature and pressure increase, and the temperature and pressure are maintained for 3h to 4h. After cooling to room temperature in the furnace, the sheath is removed to obtain a titanium alloy intermediate.

5. The method for preparing a high molybdenum equivalent metastable β titanium alloy product according to claim 4, characterized in that: In step 1), the prefabricated package is cleaned with an acetone solution and dried by heating.

6. The method for preparing a high molybdenum equivalent metastable β titanium alloy product according to claim 1, characterized in that: In step three, the solution aging treatment includes performing a solution treatment in a two-phase region and then performing an aging treatment.

7. The method for preparing a high molybdenum equivalent metastable β titanium alloy product according to claim 6, characterized in that: In the step three, the solution treatment temperature is 730°C to 780°C, and the solution treatment time is 1h to 4h; the aging treatment temperature is 510°C to 580°C, and the aging treatment time is 4h to 8h, and after the solution treatment and aging treatment, the steel is air-cooled to room temperature.

8. A high molybdenum equivalent metastable β titanium alloy product, characterized in that: The high molybdenum equivalent metastable β titanium alloy product is prepared by the preparation method described in any one of claims 1 to 7.

9. The high molybdenum equivalent metastable β titanium alloy product according to claim 8, characterized in that: The mechanical properties of the high molybdenum equivalent metastable β titanium alloy product are as follows: tensile strength ≥1300MPa, yield strength ≥1200MPa, elongation ≥10%, impact toughness ≥25J•cm -2 .

10. Use of a high molybdenum equivalent metastable β titanium alloy product prepared by the preparation method according to any one of claims 1 to 7, or a high molybdenum equivalent metastable β titanium alloy product according to claim 8 or 9 in aircraft load-bearing parts.

Citation Information

Cited By

  • Preparation method and application of short-process metastable titanium alloy

    CN119899952A