Precipitation method for separating lithium and magnesium ions in salt lake and application

By using a reaction coupling method of organic acid and water-soluble solid alkali in the salt lake simulation liquid, magnesium ions are efficiently removed and lithium ions retained, which solves the problem of low recovery rate caused by the high magnesium-lithium ratio during lithium extraction in the salt lake, and magnesium is used to remove magnesium and lithium ions. The precipitates are used for carbon dioxide adsorption, achieving efficient separation and resource reuse.

CN118993196AActive Publication Date: 2024-11-22BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202411310948.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

The method of extracting lithium in a salt lake has the problems of high magnesium-lithium ratio leading to long precipitation time, low lithium ion recovery rate, and poor ion selectivity. The traditional precipitation method is not suitable for salt lake brine with high magnesium-lithium ratio.

Method used

By adding organic acid and water-soluble solid alkali to the salt lake simulation solution for reaction coupling, the magnesium ions form a complex precipitation, thereby removing magnesium ions and leaving lithium ions in the solution. Ultrasonic heating and stirring and vacuum drying are used to achieve high efficiency. Separation.

Benefits of technology

The removal rate of magnesium is achieved up to 85-100%, and the retention rate of lithium is 96-100%. The magnesium precipitates are used as carbon dioxide adsorbents, which solves the problem of solid waste treatment and is suitable for any mixed solution of magnesium lithium ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993196A_ABST
    Figure CN118993196A_ABST
Patent Text Reader

Abstract

The invention provides a precipitation method for separating lithium and magnesium ions in a salt lake and application, and belongs to the field of separation engineering. According to the method, magnesium and lithium ions in the salt lake are separated through the coupling reaction of the organic acid and the water-soluble solid alkali, although the magnesium ions can be separated in a traditional magnesium and lithium separation method by adding the organic acid for coupling, a large number of lithium ions can be taken away in the precipitation process, so that the retention rate of the lithium ions is greatly reduced, and the separation efficiency is improved. According to the precipitation method, the removal rate of magnesium ions is high and can reach 85-100%, meanwhile, the retention rate of lithium ions is 96-100%, organic acid and water-soluble solid alkali are used in the coupling reaction process, used raw materials are green and non-toxic, the coupling process is simple, only the salt lake, the organic acid and the water-soluble solid alkali need to be added, and the organic acid and the water-soluble solid alkali are added into the coupling reaction process. The magnesium ions and the lithium ions are mixed and stirred at the specific feeding amount and temperature, the magnesium ions can be precipitated, the lithium ions are left in the solution, and the precipitation method is wide in application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of separation engineering, and specifically relates to a precipitation method for separating lithium and magnesium ions in a salt lake and an application thereof. Background Art

[0002] Lithium is the first metal element in the periodic table and one of the important metal resources. It has a wide range of uses in the nuclear energy, chemical, manufacturing and metallurgical industries. It is also the main component of new energy batteries that have been popular in recent years. Its main sources include lithium-containing ores and lithium-containing salt lake brines. There are extremely rich lithium deposits in China's salt lake brines. Compared with calcining lithium-containing ores to obtain lithium products, the method of recovering lithium from salt lake brines is relatively simple and cost-effective. However, extracting lithium from salt lakes is a global problem. my country's salt lake resources are mainly concentrated in the Qinghai-Tibet Plateau and Qinghai. Qinghai salt lakes generally have the characteristics of high magnesium-lithium ratio and low lithium content, so extraction is also very difficult.

[0003] The main methods for extracting lithium from salt lake brine include extraction, adsorption, electrodialysis and precipitation. Among them, solvent extraction is an effective method, which usually shows high selectivity for lithium ions, but the extractants are mostly organic chemicals, which cause serious corrosion to the separation equipment. Adsorbents such as layered adsorbents, aluminum salt adsorbents and ion sieves are often used in the adsorption method, but some adsorbents have problems such as easy dissolution, poor recyclability, and insufficient capacity to support industrial applications, so their actual development is hindered. Electrodialysis has been developed and attracted widespread attention due to its environmental friendliness and high efficiency in extracting lithium. However, the complex composition of the brine system and the pH value of the solution have a negative impact on the stability of the electrode, resulting in many unfavorable factors in the actual electrodialysis process. Precipitation is a traditional method for recovering lithium from salt lakes. It uses solar energy and wind energy to evaporate and concentrate salt lake brine, and separates lithium through a series of chemical reactions and physical processes. For example, CN111484046A discloses a method for extracting lithium from salt lake brine with a high magnesium-to-lithium ratio, which mainly includes taking the magnesium in the brine as a raw material, adding an aluminum source and a precipitant, precipitating the magnesium and aluminum into layered double hydroxides (MgAl-LDHs), filtering and separating, and retaining lithium ions in the filtrate, and then concentrating or ion selectively adsorbing the lithium to enrich the lithium and precipitating it with carbonate ions to obtain lithium carbonate.

[0004] CN115321705B discloses a method for separating magnesium and lithium from salt lake brine with a high magnesium-to-lithium ratio, which utilizes the selective complexing ability of complexes for alkali metal ions, and improves the interception rate of magnesium ions by nanofiltration membrane after complexing with magnesium ions, and produces lithium carbonate by concentrated precipitation. The precipitation method loses a large amount of lithium during its evaporation and precipitation process, so the overall recovery rate is not high. In addition, this method is not suitable for salt lake brine with a high magnesium-to-lithium ratio.

[0005] In summary, the method of extracting lithium from salt lakes is relatively simple in industry and has low cost. Precipitation method is often used for extraction. However, during the extraction process, due to the high magnesium-lithium ratio in some salt lakes, the precipitation time is long, the lithium ion recovery rate is low, and the ion selectivity is poor, which are still problems that need to be solved urgently. Summary of the invention

[0006] In view of the above problems, the present invention provides a precipitation method for separating lithium and magnesium ions in a salt lake and its application. The method precipitates magnesium ions in the salt lake by a reaction coupling method, while lithium ions remain in the solution, thereby separating magnesium and lithium ions. The separation process of the method is simple and the separation efficiency is high. The obtained lithium ion retention rate is high, the magnesium removal rate is high, and the impurities are small. The obtained magnesium precipitate can also be used as a carbon dioxide adsorbent, solving the problem of post-treatment of solid waste.

[0007] The invention provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises the following steps: adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 85-100% and a lithium retention rate of 96-100%.

[0008] Furthermore, the precipitation method comprises the following steps: The organic acid and the water-soluble solid base are added to the salt lake simulation liquid, and the mixture is heated and stirred after ultrasonic treatment until all the mixture is dissolved, and the heating and stirring are continued to react. After the reaction is completed, the mixture is allowed to stand to obtain a solid-liquid mixture, and the solid-liquid mixture is filtered to obtain a lithium-containing solution and a solid complex. The solid complex is washed alternately with deionized water and ethanol, and then vacuum dried. After cooling to room temperature, a magnesium precipitate is obtained.

[0009] Furthermore, the salt lake simulation liquid includes magnesium chloride, lithium chloride and deionized water.

[0010] Furthermore, the salt lake simulated liquid also includes calcium chloride, and the concentration of calcium chloride in the salt lake simulated liquid is 0.001-0.01 g / L.

[0011] Furthermore, the concentration of magnesium chloride in the salt lake simulated liquid is 4-100 g / L, and the concentration of lithium chloride is 0.01-10 g / L.

[0012] Furthermore, the mass volume ratio of the organic acid to the salt lake simulated liquid is 60-750 g / L.

[0013] Furthermore, the mass volume ratio of the water-soluble solid alkali to the salt lake simulated liquid is 25-400 g / L.

[0014] Furthermore, the organic acid is 3,4,5-trihydroxybenzoic acid, and the water-soluble solid base is potassium hydroxide.

[0015] Furthermore, the process mechanism of reaction coupling in the precipitation method is as follows: .

[0016] Furthermore, the frequency of the ultrasound is 20-50 Hz, and the time of the ultrasound is 5-20 min.

[0017] Furthermore, the temperature of the heating and stirring is 110-140° C., and the speed of the heating and stirring is 300-500 r / min.

[0018] Furthermore, the temperature of the continued heating is 110-140° C., the time of the continued heating is 12-24 hours, and the speed of the continued heating and stirring is 300-500 r / min.

[0019] Furthermore, the standing time is 0.5-1h.

[0020] Furthermore, the washing process is to wash with deionized water and ethanol for 1-3 times respectively.

[0021] Furthermore, the ethanol is 75% ethanol or anhydrous ethanol.

[0022] Furthermore, the temperature of the vacuum drying is 50-100° C., the time of the vacuum drying is 12-24 hours, and the vacuum degree of the vacuum drying is -0.08 to -0.1 MPa.

[0023] The present invention also provides a lithium-containing solution, which is prepared by the precipitation method.

[0024] The present invention also provides a lithium battery, which is prepared from the lithium-containing solution.

[0025] The present invention also provides a magnesium precipitate, which is prepared by the precipitation method and has a metal organic framework structure. In the infrared spectrum test of the magnesium precipitate, the infrared spectrum of the magnesium precipitate is 3800-2800cm -1 ±0.01cm -1 The characteristic peak of OH in the carboxyl functional group appears in the region, 1622cm -1 ±0.01cm -1 The characteristic peaks of C=O appear at 1554, 1462 and 1376 cm -1 ±0.01cm -1 The three characteristic peaks are typical stretching vibration peaks of C—C bonds in aromatic rings, 1300-1000 cm -1 ±0.01cm-1 The characteristic peaks in the region indicate the stretching vibration peaks of the CO bond and the bending vibration peaks of the OH bond in the aromatic ring, 748cm -1 ±0.01cm -1 The characteristic peak of the aromatic ring CH appears at 11.35°±0.02°, 14.05°±0.02° and 24.53°±0.02°, which correspond to the Miller index (hkl) values ​​of (010), (011) and (221), respectively. The peak position does not change after soaking, and the property is stable.

[0026] The present invention also provides an adsorbent, which includes the magnesium precipitate or is prepared from the magnesium precipitate, and is used for adsorbing carbon dioxide gas and separating carbon dioxide-methane mixed gas; at 25°C and 1.0 bar, the adsorption capacity of carbon dioxide by the adsorbent is 75-90cm 3 / g, and the separation selectivity of the adsorbent for carbon dioxide in the carbon dioxide-methane mixture is calculated to be 1600-1900 according to the adsorption isotherm by the ideal adsorption solution theory (IAST) method.

[0027] Beneficial effects of the present invention: 1. In the present invention, magnesium and lithium ions in the salt lake are separated by coupling reaction of organic acid and water-soluble solid alkali. The traditional method of separating magnesium and lithium by adding organic acid coupling can separate magnesium ions, but will take away a large amount of lithium ions during the precipitation process, which greatly reduces the retention rate of lithium ions. The precipitation method in the present invention has a high removal rate of magnesium ions, which can reach 85-100%, and the retention rate of lithium ions is also 96-100%. In addition, the organic acid and water-soluble solid alkali used in the coupling reaction process of the present invention are green and non-toxic raw materials, and the coupling process is simple. It only needs to mix and stir the salt lake, organic acid and water-soluble solid alkali at a specific feed amount and temperature to precipitate magnesium ions, while lithium ions remain in the solution. 2. The precipitation method of the present invention is simple and has good separation effect. When other interfering ions exist in the salt lake, it can still maintain a high removal rate and retention rate. It can be applied to any mixed solution of magnesium and lithium ions. The magnesium precipitate obtained after precipitation has adsorption properties, especially for a mixed gas of carbon dioxide and methane. It has good adsorption properties for carbon dioxide and high selectivity, which solves the problem of recycling the precipitate after separating magnesium and lithium. At the same time, the performance of the obtained magnesium precipitate can still remain stable under the condition of pH 2-12, and the adsorption effect of carbon dioxide is still advantageous. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The powder X-ray diffraction (PXRD) diagram of the magnesium precipitate in Example 1 after being immersed in the pH value of 2-12 for one week; Figure 2 is the infrared spectra of the magnesium precipitate in the precipitation methods of Examples 3 and 4; Figure 3 is the adsorption isotherm diagram of carbon dioxide (CO2) and methane (CH4) by the adsorbent described in Example 11; Figure 4 1 is a powder X-ray diffraction (PXRD) diagram of the magnesium precipitate in the precipitation method in Example 3 and Comparative Example 1. DETAILED DESCRIPTION

[0029] The invention is described in detail below with reference to the embodiments: The present invention discloses a precipitation method for separating lithium and magnesium ions in a salt lake and its application. The magnesium ions and lithium ions in the salt lake are separated through a simple reaction process, wherein the magnesium ions are removed by precipitation, while the lithium ions remain in the solution. The precipitation method of the method has a high removal rate of magnesium ions and a high retention rate of lithium ions.

[0030] Example 1 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 92.38% and a lithium retention rate of 98.45%.

[0031] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.25 g of 3,4,5-trihydroxybenzoic acid and 2.25 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0032] In this embodiment, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 70g / L, and the feeding amount of water-soluble solid alkali is 30g / L.

[0033] like Figure 1 The following are powder X-ray diffraction (PXRD) patterns of the magnesium precipitate in Example 1 after being soaked for one week under conditions of pH values ​​of 2-12. In the powder X-ray diffraction (PXRD), obvious diffraction peaks appear at 2θ of 11.35°±0.02°, 14.05°±0.02° and 24.53°±0.02°, corresponding to the Miller index (hkl) values ​​of (010), (011) and (221), respectively. The peak positions do not change after soaking, and the properties are stable. In the figure, the horizontal axis (2 Theta) is the diffraction angle, and the vertical axis (Intensity) is the relative intensity.

[0034] Example 2 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 89.62% and a lithium retention rate of 100%.

[0035] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.25 g of 3,4,5-trihydroxybenzoic acid and 2.63 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 110° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 110° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0036] In this embodiment, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 70g / L, and the feeding amount of water-soluble solid alkali is 35g / L.

[0037] Example 3 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 86.71% and a lithium retention rate of 98.64%.

[0038] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.25 g of 3,4,5-trihydroxybenzoic acid and 3 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 110° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 110° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0039] In this embodiment, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 70g / L, and the feeding amount of water-soluble solid alkali is 40g / L.

[0040] Example 4 This embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method is to add an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid; the precipitation method has a magnesium removal rate of 98.44% and a lithium retention rate of 100%.

[0041] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.25 g of 3,4,5-trihydroxybenzoic acid and 2.63 g of potassium hydroxide were added, and the mixture was ultrasonicated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol once, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0042] In this embodiment, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 70g / L, and the feeding amount of water-soluble solid alkali is 35g / L.

[0043] Table 1 shows the inductively coupled plasma emission spectrometry (ICP) test results of the magnesium precipitate described in Example 4.

[0044] As shown in Table 1, the lithium and magnesium ions in the salt lake simulated liquid are separated by the precipitation method of the present invention, and the lithium content in the magnesium precipitate after separation is extremely low, which proves that the precipitation method of the present invention has a small loss rate of lithium ions and a high retention rate.

[0045] like Figure 2 The infrared spectra of the magnesium precipitates in the precipitation methods of Examples 3 and 4 are shown in Figure 1. As can be seen from the figure, the magnesium precipitates in the precipitation methods of Examples 3 and 4 are all at 3800-2800cm -1 ±0.01cm -1 The characteristic peak of OH in the carboxyl functional group appears in the region, 1622cm -1 ±0.01cm -1 The characteristic peaks of C=O appear at 1554, 1462 and 1376 cm -1 ±0.01cm -1 The three characteristic peaks are typical stretching vibration peaks of C—C bonds in aromatic rings, 1300-1000 cm -1 ±0.01cm -1 The characteristic peaks in the region indicate the stretching vibration peaks of the CO bond and the bending vibration peaks of the OH bond in the aromatic ring, 748cm -1 ±0.01cm -1 The characteristic peak of aromatic ring CH appears at In the figure, the horizontal axis (Wavenumbers) is the wavelength, and the vertical axis (transmittance) is the transmittance.

[0046] Example 5 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 92.73% and a lithium retention rate of 97.83%.

[0047] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.63 g of 3,4,5-trihydroxybenzoic acid and 2.63 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0048] In this embodiment, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 75g / L, and the feeding amount of water-soluble solid alkali is 35g / L.

[0049] Example 6 This embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method is to add an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid; the precipitation method has a magnesium removal rate of 98.81% and a lithium retention rate of 100%.

[0050] In this embodiment, the precipitation method comprises the following steps: To 77 mL of the salt lake simulation liquid, 4.77 g of 3,4,5-trihydroxybenzoic acid and 2.15 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0051] In this embodiment, the salt lake simulation liquid includes 0.37g magnesium chloride, 0.0034g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 4.86g / L, the concentration of lithium chloride is 0.044g / L, and the magnesium-lithium concentration ratio is 109.73; the feeding amount of organic acid is 62g / L, and the feeding amount of water-soluble solid alkali is 28g / L.

[0052] Example 7 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 98.96% and a lithium retention rate of 96.03%.

[0053] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.01 g of 3,4,5-trihydroxybenzoic acid and 2.31 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0054] In this embodiment, the salt lake simulation liquid includes 0.37g magnesium chloride, 0.36g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 4.95g / L, the concentration of lithium chloride is 4.82g / L, and the magnesium-lithium concentration ratio is 1.03; the feeding amount of organic acid is 65g / L, and the feeding amount of water-soluble solid alkali is 30g / L.

[0055] Example 8 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 99.63% and a lithium retention rate of 97.14%.

[0056] In this embodiment, the precipitation method comprises the following steps: To 80 mL of the salt lake simulation liquid, 10.4 g of 3,4,5-trihydroxybenzoic acid and 4.8 g of potassium hydroxide were added, and the mixture was ultrasonicated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0057] In this embodiment, the salt lake simulation liquid includes 0.79g magnesium chloride, 0.0028g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 9.86g / L, the concentration of lithium chloride is 0.035g / L, and the magnesium-lithium concentration ratio is 281.71; the feeding amount of organic acid is 130g / L, and the feeding amount of water-soluble solid alkali is 60g / L.

[0058] Example 9 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 98.71% and a lithium retention rate of 99.85%.

[0059] In this embodiment, the precipitation method comprises the following steps: To 100 mL of the salt lake simulation liquid, add 70 g of 3,4,5-trihydroxybenzoic acid and 35 g of potassium hydroxide, and after ultrasonication at 20 Hz for 10 min, heat and stir at 130° C. and 300 r / min until all dissolved, continue heating at 130° C. and 300 r / min for 12 h to react, stand for 0.5 h after the reaction to obtain a solid-liquid mixture, filter the solid-liquid mixture to obtain a lithium-containing solution and a solid complex, wash the solid complex alternately with deionized water and anhydrous ethanol twice, vacuum dry it at 80° C. and −0.1 MPa for 12 h, and cool it to room temperature to obtain a magnesium precipitate.

[0060] In this embodiment, the salt lake simulation liquid includes 7.659g magnesium chloride, 0.0268g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 76.59g / L, the concentration of lithium chloride is 0.268g / L, and the magnesium-lithium concentration ratio is 285.78; the feeding amount of organic acid is 700g / L, and the feeding amount of water-soluble solid alkali is 350g / L.

[0061] Example 10 The present embodiment provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid. The precipitation method has a magnesium removal rate of 97.20% and a lithium retention rate of 99.26%.

[0062] In this embodiment, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.25 g of 3,4,5-trihydroxybenzoic acid and 2.63 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 130° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 130° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0063] In this embodiment, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride, 0.00045g calcium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, the concentration of calcium chloride is 0.006g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 70g / L, and the feeding amount of water-soluble solid alkali is 35g / L.

[0064] Embodiment 11 The present invention also provides an adsorbent, which includes the magnesium precipitate described in Example 1, and is used for adsorbing carbon dioxide gas and separating carbon dioxide-methane mixed gas; at 25°C and 1.0 bar, the adsorption capacity of carbon dioxide by the adsorbent is 81.56 cm 3 / g, and the separation selectivity of the adsorbent for carbon dioxide in the carbon dioxide-methane mixture is calculated to be 1753 according to the adsorption isotherm using the ideal adsorption solution theory (IAST) method.

[0065] like Figure 3 The adsorption isotherms of carbon dioxide (CO2) and methane (CH4) of the adsorbent in Example 11 are shown in the figure. It can be seen from the figure that the adsorbent has good adsorption of carbon dioxide, and the adsorption amount is 81.56 cm 3 / g, therefore, carbon dioxide and methane can be separated, and the separation selectivity of carbon dioxide can reach 1753; In the figure, the horizontal axis (P / P0) is the relative pressure, and the vertical axis (Gas uptake) is the adsorption amount; The testing process of the adsorption isotherm is as follows: 100 mg of the adsorbent was activated at 80° C. for 12 h, the activated adsorbent was degassed and loaded into a sample tube, and carbon dioxide and methane gases were introduced into the sample tube containing the adsorbent using a BSD-660M A6M high-performance gas adsorption and micropore analyzer, and the adsorption performance of the adsorbent was tested at 25° C. and 1.0 bar.

[0066] Comparative Example 1 This comparative example provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid; the precipitation method has a magnesium removal rate of 71.66% and a lithium retention rate of 96.65%.

[0067] In this comparative example, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 5.25 g of 3,4,5-trihydroxybenzoic acid and 2.25 g of potassium hydroxide were added, and the mixture was ultrasonically treated at 20 Hz for 10 min, and then heated and stirred at 170° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 170° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0068] In this comparative example, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 70g / L, and the feeding amount of water-soluble solid alkali is 30g / L.

[0069] like Figure 4 The figure is a powder X-ray diffraction (PXRD) diagram of the magnesium precipitate in the precipitation method in Example 3 and Comparative Example 1. It can be seen from the figure that the magnesium precipitate in Comparative Example 1 has a small amount of impurity peaks and peak fluctuations compared with Example 3, indicating that there are partial defects in its crystal structure; In the figure, the horizontal axis (2 Theta) is the diffraction angle, and the vertical axis (Intensity) is the relative intensity.

[0070] Comparative Example 2 This comparative example provides a precipitation method for separating lithium and magnesium ions in a salt lake. The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid; the precipitation method has a magnesium removal rate of 69.96% and a lithium retention rate of 93.51%.

[0071] In this comparative example, the precipitation method comprises the following steps: To 75 mL of the salt lake simulation liquid, 6.75 g of 3,4,5-trihydroxybenzoic acid and 3.75 g of potassium hydroxide were added, and the mixture was ultrasonicated at 20 Hz for 10 min, and then heated and stirred at 110° C. and 300 r / min until all the mixture was dissolved. The mixture was heated at 110° C. and 300 r / min for 12 h to react. After the reaction was completed, the mixture was allowed to stand for 0.5 h to obtain a solid-liquid mixture, and the solid-liquid mixture was filtered to obtain a lithium-containing solution and a solid complex. The solid complex was washed alternately with deionized water and anhydrous ethanol twice, and then vacuum dried at 80° C. and −0.1 MPa for 12 h, and cooled to room temperature to obtain a magnesium precipitate.

[0072] In this comparative example, the salt lake simulation liquid includes 0.45g magnesium chloride, 0.0055g lithium chloride and deionized water, wherein the concentration of magnesium chloride is 6g / L, the concentration of lithium chloride is 0.073g / L, and the magnesium-lithium concentration ratio is 82.19; the feeding amount of organic acid is 90g / L, and the feeding amount of water-soluble solid alkali is 50g / L.

[0073] Table 2 is the data of the precipitation method in Examples 1-10 and Comparative Examples 1-2

[0074] As shown in Table 2, the test results of the precipitation method described in Examples 1-10 and Comparative Examples 1-2 are shown. It can be seen from the table that when the magnesium content in the salt lake simulated liquid increases (Example 6, Example 8 and Example 9) or when other interfering ions exist in the salt lake simulated liquid (Example 10), the precipitation method of the present invention can still better separate magnesium and lithium ions, with a high magnesium removal rate and a high lithium ion retention rate; while in Comparative Examples 1 and 2, the temperature is increased or the amount of organic acid and water-soluble solid alkali added is excessively increased, resulting in insufficient reaction, and thus the magnesium removal rate is reduced.

[0075] Based on the above, it can be seen that the precipitation method of the present invention has a wide range of applications, low cost, and extremely high market prospects.

[0076] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.

Claims

1. A precipitation method for separating lithium and magnesium ions in salt lakes, It is characterized in that The precipitation method comprises adding an organic acid and a water-soluble solid base to a salt lake simulation liquid for reaction coupling, so that the magnesium ions in the salt lake simulation liquid form a complex precipitate with the organic acid and the water-soluble solid base, thereby removing the magnesium ions in the salt lake simulation liquid; the precipitation method has a magnesium removal rate of 85-100% and a lithium retention rate of 96-100%.

2. The precipitation method according to claim 1, It is characterized in that The precipitation method comprises the following steps: The organic acid and the water-soluble solid base are added to the salt lake simulation liquid, and the mixture is heated and stirred after ultrasonic treatment until all the mixture is dissolved, and the heating and stirring are continued to react. After the reaction is completed, the mixture is allowed to stand to obtain a solid-liquid mixture, and the solid-liquid mixture is filtered to obtain a lithium-containing solution and a solid complex. The solid complex is washed alternately with deionized water and ethanol, and then vacuum dried. After cooling to room temperature, a magnesium precipitate is obtained.

3. The precipitation method according to claim 1, It is characterized in that The salt lake simulation liquid includes magnesium chloride, lithium chloride and deionized water.

4. The precipitation method according to claim 1, It is characterized in that The concentration of magnesium chloride in the salt lake simulation liquid is 4-100 g / L, and the concentration of lithium chloride is 0.01-10 g / L.

5. The precipitation method according to claim 1, It is characterized in that The mass volume ratio of the organic acid to the salt lake simulated liquid is 60-750 g / L.

6. The precipitation method according to claim 1, It is characterized in that The mass volume ratio of the water-soluble solid alkali to the salt lake simulated liquid is 25-400 g / L.

7. The precipitation method according to claim 1, It is characterized in that The organic acid is 3,4,5-trihydroxybenzoic acid, and the water-soluble solid base is potassium hydroxide.

8. The precipitation method according to claim 2, It is characterized in that The heating and stirring temperature is 110-140° C., and the heating and stirring speed is 300-500 r / min.

9. A magnesium precipitate, It is characterized in that The magnesium precipitate is prepared by the precipitation method according to any one of claims 1 to 8; the magnesium precipitate is a metal organic framework structure; in the infrared spectrum test of the magnesium precipitate, the infrared spectrum of the magnesium precipitate is 3800-2800cm -1 ±0.01cm -1 The characteristic peak of OH in the carboxyl functional group appears in the region, 1622cm -1 ±0.01cm -1 The characteristic peaks of C=O appear at 1554, 1462 and 1376 cm -1 ±0.01cm -1 The three characteristic peaks are typical stretching vibration peaks of C—C bonds in aromatic rings, 1300-1000 cm -1 ±0.01cm -1 The characteristic peaks in the region indicate the stretching vibration peaks of the CO bond and the bending vibration peaks of the OH bond in the aromatic ring, 748cm -1 ±0.01cm -1 The characteristic peak of the aromatic ring CH appears at 11.35°±0.02°, 14.05°±0.02° and 24.53°±0.02° in powder X-ray diffraction after the magnesium precipitate is soaked for one week under the condition of pH value of 2-12, which corresponds to the Miller index values ​​of (010), (011) and (221) respectively. The peak position does not change after soaking, and the property is stable.

10. An adsorbent, It is characterized in that The adsorbent comprises the magnesium precipitate according to claim 9 or is prepared from the magnesium precipitate according to claim 9, and the adsorbent is used for adsorbing carbon dioxide gas and separating carbon dioxide-methane mixed gas; at 25°C and 1.0 bar, the adsorption capacity of carbon dioxide by the adsorbent is 75-90cm 3 / g, and the separation selectivity of the adsorbent for carbon dioxide in the carbon dioxide-methane mixture is calculated to be 1600-1900 according to the ideal adsorption solution theory method and the adsorption isotherm.

Citation Information

Patent Citations

  • Novel method for preparing bicyclol

    CN102617544A

  • Metal-organic framework material for methane adsorption separation and preparation method thereof

    CN102962037A

  • Method for isolating magnesium and lithium from solution containing magnesium and lithium

    CN106629790A

  • Method for purifying and treating wastewater in production process of gallic acid by nano hydrogel material

    CN106745593A

  • Metal organic frame material for separating ethane and ethylene and separation method of ethylene and ethane

    CN108014752A

Cited By

  • Selective separation process of sodium-potassium mixed salt

    CN121107438A