Carbon bowl roasting filler and filling method
By mixing metallurgical coke, sawdust and adhesive specific ratios, the charcoal bowl roasting filler formed solves the problem of bonding after roasting and the problem of short storage time of filling, achieving stable shape after long-term storage and roasting Effective, and metallurgical coke can be recycled.
Patent Information
- Application Number
- CN202411185167.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
The existing charcoal bowl roasting filler bonds to the charcoal bowl after roasting, resulting in defects in the charcoal bowl, and the filling material is stored for a short time and cannot be stored for a long time.
Metallurgical coke, sawdust and adhesive are mixed in a specific proportion to form a charcoal bowl roasted filler. Metallurgical coke provides support. The sawdust has water absorption and combustion-enhancing functions. The adhesive extends the moisture and does not evaporate easily and extends the storage time of the filler.
It extends the storage time of the filler, is easy to remove after roasting, and ensures the shaping effect of the charcoal bowl. The metallurgical coke can be recycled and recycled. The filling material is simple and easy to obtain, and the storage time is long.
Smart Images

Figure CN118993636A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of carbon in the metallurgical industry, and in particular to a charcoal bowl roasting filler and a filling method. Background Art
[0002] In the production process of aluminum electrolysis prebaked anode carbon blocks, in order to prevent the carbon bowl from collapsing and deforming during roasting, the carbon bowl must be pre-filled before the carbon blocks are assembled and loaded into the furnace to play a supporting role. To address this problem, metallurgical coke or petroleum coke is currently mainly used for direct filling, but the filler may form a bond with the carbon bowl after sintering, causing defects to the carbon bowl. In addition, when mixed fillers are used, most of them need to be prepared and used immediately, and cannot be stored for a long time. Summary of the invention
[0003] The present application provides a charcoal bowl roasting filler and a filling method to solve the following technical problem: prolonging the storage time of the filler.
[0004] In a first aspect, the present invention provides a charcoal bowl roasted filler. The raw materials of the charcoal bowl roasted filler include, by mass fraction: 25% to 55% metallurgical coke, 25% to 45% sawdust, 20% to 30% water and 0% to 15% adhesive.
[0005] Optionally, the metallurgical coke is 30% to 45%, the sawdust is 30% to 45%, the water is 20% to 30%, and the binder is 5% to 15%.
[0006] Optionally, the adhesive comprises a mixture of one or more of gum secreted by trees, rare earth adhesives, clay adhesives and plant starch.
[0007] Optionally, the particle size of the metallurgical coke is 20 mm to 40 mm.
[0008] Optionally, the particle size of the sawdust is not greater than 10 mm.
[0009] Optionally, the moisture content of the sawdust is not more than 38%.
[0010] In a second aspect, the present invention further provides a method for filling a charcoal bowl with a roasted filler, using the charcoal bowl roasted filler provided in the first aspect, the method comprising the following steps:
[0011] Prepare charcoal bowl roasting filling;
[0012] The filler is filled into the charcoal bowl until the filler is flush with the bowl mouth of the charcoal bowl.
[0013] Optionally, the preparation of the charcoal bowl roasted filler specifically includes: uniformly mixing metallurgical coke, sawdust, water and a binder according to the mass fractions to obtain the charcoal bowl roasted filler.
[0014] Optionally, the charcoal bowl roasted filling material can be stored for 8 hours to 24 hours.
[0015] The above technical solution provided by the present invention has the following advantages compared with the prior art:
[0016] The present invention provides a charcoal bowl roasted filler and a filling method. The filler raw materials include: 25% to 55% metallurgical coke, 25% to 45% sawdust, 20% to 30% water and 0% to 15% adhesive. Metallurgical coke, as a granular fuel with high carbon content, can play a role in material shaping and supporting in the filler, and will not change after roasting, and can be recycled and reused; sawdust is small and fine wood chips made from wood processing, which has the functions of water absorption, toughness and combustion support. After the water-absorbing sawdust is mixed with metallurgical coke, water is added and compacted, and the filler is shaped in the charcoal bowl. The adhesive makes it difficult for the water in the filler to evaporate, maintains the moisture for a long time, and prolongs the storage time of the filler.
[0017] The raw material components of the filler are simple and easy to obtain, and the storage time is long; it is easy to remove after roasting, ensuring the roasting shaping effect of the charcoal bowl, and the metallurgical coke can be recycled and reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0019] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0020] Figure 1 A flow chart of a method for filling a charcoal bowl with roasted filling material provided in some embodiments of the present application. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0022] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0023] In this application, in the absence of any contrary description, the terms including "including" and the like mean "including but not limited to". In this article, relational terms such as "first" and "second" and the like are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plurality" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions thereof refer to any combination of these items, including any combination of singular (individual) or plural (individual). For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0024] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0025] In a first aspect, the present invention provides a charcoal bowl roasted filler. The raw materials of the charcoal bowl roasted filler include, by mass fraction: 25% to 55% metallurgical coke, 25% to 45% sawdust, 20% to 30% water and 0% to 15% adhesive.
[0026] In the above embodiment, metallurgical coke, as a granular fuel with high carbon content, can play a role in shaping and supporting the material in the filler, and will not change after roasting, and can be recycled; sawdust is small and fine wood chips made from wood processing, which has the functions of water absorption, toughness and combustion support. After the water-absorbing sawdust is mixed with metallurgical coke, water is added and compacted, the filler is shaped in the charcoal bowl. The adhesive makes it difficult for the water in the filler to evaporate, maintains the moisture for a long time, and prolongs the storage time of the filler.
[0027] As an optional implementation, the metallurgical coke is 30% to 45%, the sawdust is 30% to 45%, the water is 20% to 30% and the binder is 5% to 15%.
[0028] In the above embodiment, the ratio of each component is further optimized, so that the storage time of the filling material is longer and the roasting effect is more stable.
[0029] As an optional embodiment, the adhesive comprises a mixture of one or more of gum secreted by trees, rare earth adhesives, clay adhesives and plant starch.
[0030] In the above embodiment, the role of the adhesive is to bond the metallurgical coke and sawdust in the filler more tightly. The selected adhesive can be an adhesive naturally existing in nature, such as rubber liquid secreted by rubber trees, and adhesive products including rubber liquid; corn starch in plant starch, etc., or adhesive products containing starch can also be used; existing rare earth adhesives and clay adhesives can also be used.
[0031] As an optional implementation manner, the particle size of the metallurgical coke is 20 mm to 40 mm.
[0032] The particle size of metallurgical coke is related to the molding of the filler. Therefore, in the above embodiment, the particle size of the metallurgical coke needs to be controlled. If the particle size is too large, it is difficult to mix evenly with the sawdust and the bonding is insufficient. If the particle size is too small, it cannot play a supporting role in the filler to maintain the hardness and stability of the filler. Therefore, the particle size needs to be controlled to be 20mm to 40mm. For example, the particle size of the metallurgical coke can be 20mm, 25mm, 30mm, 35mm or 40mm.
[0033] As an optional implementation, the particle size of the sawdust is not greater than 10 mm.
[0034] In the above embodiment, the sawdust particle size also affects the molding effect of the filler. If the sawdust particle size is too large, it cannot be well wrapped on the surface of the metallurgical coke after absorbing water, resulting in poor stability of the filler. Therefore, the sawdust particle size is controlled to be no more than 10 mm. Exemplarily, the sawdust particle size can be 10 mm, 9 mm, 8 mm, 7 mm, 6 mm, 5 mm, 4 mm, 3 mm or 2 mm.
[0035] As an optional implementation manner, the moisture content of the sawdust is not more than 38%.
[0036] In the above embodiment, the water content of the sawdust is controlled because when the water content of the sawdust is too high, it is easy to form lumps, has poor fluidity, and is difficult to stir, resulting in uneven mixing when mixed with metallurgical coke, affecting the stability of the filler.
[0037] In a second aspect, the present invention further provides a method for filling a charcoal bowl with a roasted filler, using the filler described in the first aspect, comprising the following steps:
[0038] Prepare charcoal bowl roasting filling;
[0039] The filler is filled into the charcoal bowl until the filler is flush with the bowl mouth of the charcoal bowl.
[0040] In the above embodiment, a charcoal bowl roasting filler is prepared and filled into the charcoal bowl until the bowl mouth is flush, so that the filler fully fills the internal space of the charcoal bowl, thereby being able to support the charcoal bowl without deformation during roasting.
[0041] As an optional implementation manner, the preparation of the charcoal bowl roasting filler specifically includes: mixing metallurgical coke, sawdust, water and a binder uniformly according to a mass ratio to obtain the charcoal bowl roasting filler.
[0042] In the above embodiment, the filler material according to the specific mass ratio can satisfy the supporting function, be easy to clean after the baking is completed, and extend the storage time of the filler material.
[0043] As an optional implementation, preparing the charcoal bowl roasted filler specifically includes: adding metallurgical coke, sawdust, water and adhesive into a mixer in sequence according to mass ratio, and stirring for more than 3 minutes to mix the raw materials of the filler evenly, thereby obtaining the charcoal bowl roasted filler.
[0044] As an optional implementation, the method for filling the charcoal bowl with roasted filler also includes: compacting the filler in the charcoal bowl.
[0045] In the above embodiment, the filling material in the charcoal bowl is compacted to further increase the supporting effect of the filling material. The compaction method can be performed using a compaction mechanism.
[0046] As an optional implementation, the charcoal bowl roasted filling material can be stored for 8 hours to 24 hours.
[0047] In the above embodiment, the combination of metallurgical coke, sawdust and water in the filler obtained in the present application makes the filler easy to shape and can play a supporting role. In addition, due to the addition of the binder, the water in the filler is not easy to volatilize, and the filler has a long storage time. Usually, after being stored for 8 to 24 hours, its roasting effect has almost no change. If the storage time is longer, the roasting effect is poor, but it can still play a certain supporting effect.
[0048] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0049] Example 1
[0050] The present embodiment provides a charcoal bowl roasting filler, the raw materials of which include, by mass fraction, 25% metallurgical coke, 45% sawdust, 25% water, and 5% adhesive.
[0051] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0052] According to the mass ratio of 25% metallurgical coke, 45% sawdust, 25% water and 5% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and stirred for more than 3 minutes and then mixed evenly to obtain a charcoal bowl roasting filler;
[0053] The charcoal bowl is filled with the charcoal bowl roasting filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed charcoal block, and the formed charcoal block can be waited for roasting.
[0054] After experiments, it was found that the filled charcoal bowl, i.e. the formed charcoal block, can be loaded into the furnace for roasting at any time; after the formed charcoal blocks were stored for 8 hours, the filling stability of the formed charcoal blocks was tested, and the test results showed that 95% of the formed charcoal blocks had qualified filling effects and met the roasting requirements.
[0055] Example 2
[0056] The present embodiment provides a charcoal bowl roasting filler, the raw materials of which include, by mass fraction, 35% metallurgical coke, 35% sawdust, 25% water, and 5% adhesive.
[0057] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0058] According to the mass ratio of 35% metallurgical coke, 35% sawdust, 25% water and 5% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 5 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0059] The charcoal bowl is filled with the charcoal bowl roasting filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed charcoal block, and the formed charcoal block can be waited for roasting.
[0060] After experiments, it was found that the filled charcoal bowl, i.e. the shaped carbon block, can be loaded into the furnace for roasting at any time; after the shaped carbon block was stored for 10 hours, the filling stability of the shaped carbon block was tested again. The test results showed that 92% of the shaped carbon blocks had qualified filling effects and met the roasting requirements.
[0061] Example 3
[0062] The present embodiment provides a charcoal bowl roasting filler, the raw materials of which include, by mass fraction, 35% metallurgical coke, 35% sawdust, 22% water, and 8% binder.
[0063] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0064] According to the mass ratio of 35% metallurgical coke, 35% sawdust, 22% water and 8% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 3 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0065] The charcoal bowl is filled with the charcoal bowl roasting filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed charcoal block, and the formed charcoal block can be waited for roasting.
[0066] After experiments, it was found that the filled charcoal bowl, i.e. the formed carbon block, can be loaded into the furnace for roasting at any time. After the formed carbon block was stored for 12 hours, the filling stability of the formed carbon block was tested. The test results showed that 93% of the formed carbon blocks had qualified filling effects and met the roasting requirements.
[0067] Example 4
[0068] The present embodiment provides a charcoal bowl roasting filler, the raw materials of which include, by mass fraction, 30% metallurgical coke, 35% sawdust, 20% water, and 15% binder.
[0069] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0070] According to the mass ratio of 30% metallurgical coke, 35% sawdust, 20% water and 15% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and the mixture is stirred for 3 minutes and then evenly mixed to obtain a charcoal bowl roasting filler;
[0071] The charcoal bowl is filled with the charcoal bowl roasting filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed charcoal block, and the formed charcoal block can be waited for roasting.
[0072] After experiments, it was found that the filled charcoal bowl, i.e. the formed charcoal block, can be loaded into the furnace for roasting at any time. After the formed charcoal blocks were stored for 24 hours, the filling stability of the formed charcoal blocks was tested. The test results showed that 90% of the formed charcoal blocks had qualified filling effects and met the roasting requirements.
[0073] Example 5
[0074] The present embodiment provides a charcoal bowl roasting filler, wherein the raw materials thereof include, by mass fraction, 35% metallurgical coke, 30% sawdust, 20% water, and 8% binder.
[0075] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0076] According to the mass ratio of 35% metallurgical coke, 30% sawdust, 20% water and 8% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 3 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0077] The charcoal bowl is filled with the charcoal bowl roasting filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed charcoal block, and the formed charcoal block can be waited for roasting.
[0078] Experimental tests have shown that the filled charcoal bowls, i.e. the formed charcoal blocks, can be loaded into the furnace for roasting at any time. After the formed charcoal blocks have been stored for 12 hours, the filling stability of the formed charcoal blocks is tested, and the test results show that 94% of the formed charcoal blocks have qualified filling effects and meet the roasting requirements.
[0079] Example 6
[0080] The present embodiment provides a charcoal bowl roasting filler, wherein the raw materials thereof include, by mass fraction, 50% metallurgical coke, 20% sawdust, 30% water, and 0% adhesive.
[0081] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0082] According to the mass ratio of 50% metallurgical coke, 20% sawdust, 30% water and 0% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 3 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0083] The charcoal bowl is filled with the charcoal bowl roasting filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed charcoal block, and the formed charcoal block can be waited for roasting.
[0084] The experimental test found that the filled carbon bowl, i.e. the formed carbon block, can be loaded into the furnace for roasting at any time. After the formed carbon block was stored for 3 hours, the filling stability of the formed carbon block was tested. The test results showed that 80% of the formed carbon blocks had a qualified filling effect and met the roasting requirements.
[0085] Comparative Example 1
[0086] This comparative example provides a charcoal bowl roasting filler, and its raw materials include, by mass fraction: 20% metallurgical coke, 45% sawdust, 20% water, and 5% adhesive.
[0087] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0088] According to the mass ratio of 20% metallurgical coke, 45% sawdust, 20% water and 5% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 3 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0089] Since the metallurgical coke content in the filler is low and the sawdust content is high, there is a problem of high compaction elasticity. Therefore, the charcoal bowl is filled with the roasted filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed carbon block. It was found that only 85% of the formed carbon blocks met the furnace loading standards; when the formed carbon blocks were stored for 3 hours, the qualified rate was reduced to 75%.
[0090] Comparative Example 2
[0091] This comparative example provides a charcoal bowl roasting filler, and its raw materials include, by mass fraction, 55% metallurgical coke, 20% sawdust, 20% water, and 5% adhesive.
[0092] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0093] According to the mass ratio of 55% metallurgical coke, 20% sawdust, 20% water and 5% binder, metallurgical coke, sawdust, water and binder are weighed respectively, the above raw materials are mixed, and the mixture is stirred for 3 minutes and then mixed evenly to obtain a charcoal bowl roasting filler;
[0094] Since the metallurgical coke content in the filler is relatively high and it is difficult to compact, the charcoal bowl is filled with the roasted filler until the bowl mouth is flush, and then the filler is compacted by a compacting mechanism to obtain a formed carbon block. Only 65% of the formed carbon blocks meet the furnace loading standards; after the formed carbon blocks are stored for 8 hours, the qualified rate is reduced to 45%.
[0095] Comparative Example 3
[0096] This comparative example provides a charcoal bowl roasting filler, and its raw materials include, by mass fraction, 35% metallurgical coke, 35% sawdust, 15% water, and 15% adhesive.
[0097] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0098] According to the mass ratio of 35% metallurgical coke, 35% sawdust, 15% water and 15% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 3 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0099] Since the water content in the filler is low, the filler mixture of metallurgical coke and sawdust is not easy to agglomerate, so the charcoal bowl is filled with the calcined filler until the bowl mouth is flush, and then compacted by a compacting mechanism to obtain a formed carbon block. Only 75% of the formed carbon blocks meet the furnace loading standards. After the formed carbon blocks are stored for 10 hours, the qualified rate is reduced to 65%.
[0100] Comparative Example 4
[0101] This comparative example provides a charcoal bowl roasting filler, and its raw materials include, by mass fraction, 25% metallurgical coke, 50% sawdust, 15% water, and 15% adhesive.
[0102] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0103] According to the mass ratio of 25% metallurgical coke, 50% sawdust, 15% water and 15% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and stirred for more than 3 minutes to obtain a charcoal bowl roasting filler;
[0104] Since the sawdust content in the filler is relatively high, there is a problem of high compaction elasticity. Therefore, the charcoal bowl is filled with the roasted filler until the bowl mouth is flush, and a formed carbon block is obtained after compaction by a compaction mechanism. Only 75% of the formed carbon blocks meet the furnace loading standards. After the formed carbon blocks are stored for 10 hours, the qualified rate is reduced to 65%.
[0105] Comparative Example 5
[0106] This comparative example provides a charcoal bowl roasting filler, and its raw materials include, by mass fraction: 35% metallurgical coke, 25% sawdust, 35% water, and 5% adhesive.
[0107] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0108] According to the mass ratio of 35% metallurgical coke, 25% sawdust, 35% water and 5% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, stirring for more than 3 minutes, and the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0109] Due to the high water content in the filler, the material is too sparse and difficult to shape, so the charcoal bowl is filled with the roasted filler until the bowl mouth is flush, and then compacted by a compacting mechanism to obtain a formed carbon block. Only 25% of the formed carbon blocks meet the furnace loading standards. After the formed carbon blocks are stored for 24 hours, the water content in the filler decreases, and the qualified rate of the formed carbon blocks rises to 60%.
[0110] Comparative Example 6
[0111] This comparative example provides a charcoal bowl roasting filler, and its raw materials include, by mass fraction, 56% metallurgical coke, 25% sawdust, 15% water, and 4% adhesive.
[0112] The method of using the above-mentioned charcoal bowl roasting filler to fill the charcoal bowl comprises the following steps:
[0113] According to the mass ratio of 56% metallurgical coke, 25% sawdust, 15% water and 4% binder, metallurgical coke, sawdust, water and binder are weighed respectively, and the above raw materials are added into a stirring mechanism for mixing, and after stirring for 3 minutes, the mixture is evenly mixed to obtain a charcoal bowl roasting filler;
[0114] Since the filler contains a high content of metallurgical coke and a low content of water, the filler is too dry and cannot be compacted. Therefore, the charcoal bowl is filled with the roasted filler until the bowl mouth is flush with the filler. After compaction by a compacting mechanism, a formed carbon block is obtained. Only 25% of the formed carbon blocks meet the furnace loading standards. After the formed carbon blocks are placed for 24 hours, the water content in the filler is further reduced, and the qualified rate is less than 20%.
[0115] In summary, it can be seen from the experimental results of the embodiments and comparative examples that the formed carbon blocks prepared by the fillers and filling methods in the present application in the embodiments can be directly roasted. Moreover, even if the formed carbon blocks in Examples 1 to 5 are stored for more than 8 hours, more than 90% of the formed carbon blocks still meet the roasting standards. However, since the raw material ratio of the filler in the comparative example does not meet the raw material ratio of the filler provided in the present invention, the filling and molding effect of the charcoal bowl is not good, and the qualified rate for roasting is significantly lower than that in the embodiments.
[0116] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A charcoal bowl roasting filler, characterized in that: Calculated by mass fraction, the raw materials of the charcoal bowl roasting filler include: 25% to 55% of metallurgical coke, 25% to 45% of sawdust, 20% to 30% of water and 0% to 15% of adhesive.
2. The charcoal bowl roasting filler according to claim 1, characterized in that: The metallurgical coke accounts for 30% to 45%, the sawdust accounts for 30% to 45%, and the adhesive accounts for 5% to 15%.
3. The charcoal bowl roasting filler according to claim 1, characterized in that: The adhesive comprises a mixture of one or more of gum secreted by trees, rare earth adhesive, clay adhesive and plant starch.
4. The charcoal bowl roasting filler according to claim 1, characterized in that: The particle size of the metallurgical coke is 20 mm to 40 mm.
5. The charcoal bowl roasting filler according to claim 1, characterized in that: The particle size of the sawdust is no greater than 10 mm.
6. The charcoal bowl roasting filler according to claim 5, characterized in that: The moisture content of the sawdust is not more than 38%.
7. A method for filling a charcoal bowl with the charcoal bowl roasting filler according to any one of claims 1 to 6, characterized in that: The following steps are involved: Prepare charcoal bowl roasting filling; The filler is filled into the charcoal bowl until the filler is flush with the bowl mouth of the charcoal bowl.
8. The filling method according to claim 7, characterized in that: The preparation of the charcoal bowl roasted filler specifically comprises: mixing metallurgical coke, sawdust, water and a binder evenly according to the mass fractions to obtain the charcoal bowl roasted filler.
Citation Information
Cited By
Pre-baked anode green body carbon bowl filler for aluminum and preparation method of pre-baked anode green body carbon bowl filler
CN121181363A