Anti-ultraviolet artificial leather surface treating agent and preparation method thereof
The anti-UV artificial leather surface treatment agent prepared by using benzophenone compounds, benzotriazole compounds and triazine compounds as UV absorbers and combined with ethylenediaminetetraacetic acid as free radical scavengers, has solved the problem of current situation There is a problem of insufficient anti-ultraviolet ability in the technology, which significantly extends the service life of the leather and improves its anti-ultraviolet aging ability.
Patent Information
- Application Number
- CN202410952092.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to develop an UV-resistant artificial leather surface treatment agent with good UV resistance, which cannot effectively absorb UV rays and prevent leather aging and cracks.
Benzophenone compounds, benzotriazole compounds, and triazine compounds are used as UV absorbers, and ethylenediaminetetraacetic acid and its derivatives are used as free radical scavengers, combining polyester polyols, diisocyanates and Organotin catalyst, preparation of UV-resistant artificial leather surface treatment agent.
Effectively absorb ultraviolet rays, reduce the aging and cracks of leather, extend the service life of leather, and improve its resistance to UV aging.
Smart Images

Figure BDA0004947509380000031 
Figure BDA0004947509380000041 
Figure BDA0004947509380000042
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment agent production, in particular to an anti-ultraviolet artificial leather surface treatment agent and a preparation method thereof. Background Art
[0002] Artificial leather is an important alternative to natural leather because of its obvious advantages in durability, appearance and feel. However, artificial leather also needs to face the problem of ultraviolet rays in daily use. Ultraviolet rays are a kind of solar radiation. Long-term exposure to ultraviolet rays will cause artificial leather to fade and deteriorate. In order to solve this problem, it is particularly important to treat artificial leather with anti-ultraviolet rays. Anti-ultraviolet treatment of artificial leather can extend its service life. Ultraviolet rays are a major natural enemy of artificial leather. Long-term exposure to ultraviolet rays will cause the surface of artificial leather to fade and discolor, affecting the appearance and quality of the product. Artificial leather treated with anti-ultraviolet rays can better resist the damage of ultraviolet rays in daily use, extend its service life, and save consumers more money and energy. In addition, anti-ultraviolet treatment can also maintain the appearance and feel of artificial leather. The impact of ultraviolet rays on the surface of artificial leather will cause it to discolor and fade, reducing the beauty and added value of the product. Artificial leather treated with anti-ultraviolet rays can better maintain its original color and appearance, extending the beauty and service life of the product. Most importantly, anti-ultraviolet treatment is of great significance to environmental friendliness and sustainable development. Traditional leather production processes produce a large amount of chemical wastewater and waste, causing serious environmental pollution. The production of artificial leather is more environmentally friendly. After UV protection treatment, it can extend its service life, reduce the impact on the environment, and promote sustainable development.
[0003] In general, the importance of anti-ultraviolet treatment of artificial leather cannot be ignored. This not only prolongs the service life of the product and maintains its appearance and feel, but also promotes environmental protection and sustainable development. Therefore, in the production process of artificial leather, anti-ultraviolet treatment of the product is an indispensable measure to provide consumers with a better product experience and environmentally friendly choices.
[0004] Chinese patent application 201710346840.7 discloses a leather surface treatment agent and its preparation method. The modified rapeseed oil and epoxy soybean oil modified polyurethane resin in the leather treatment agent provided by the scheme can effectively penetrate into the leather, so that the leather absorbs a certain amount of oil, has strong ultraviolet absorption performance, and the finished leather has a good oily feel after greasing, which effectively prevents the leather from being hardened and cracked, and is worthy of promotion and use; on the other hand, Al2O3 sol-modified waste leather micropowder forms a polymer with a double-layer nanolayer, so that the coating on the surface of the leather treated with the surface treatment agent has more stable and lasting super strong water-repellent, oil-repellent, and anti-fouling properties; the nanoparticles that come into contact with the original surface of the leather can be deeply combined with the concave and convex of the original surface, further increasing the connection between the coating and the leather, so that oil or water cannot directly penetrate into the leather, greatly improving the water-repellent, oil-repellent and anti-fouling properties;
[0005] This solution uses modified rapeseed oil and epoxidized soybean oil to modify polyurethane resin, allowing the leather to absorb a certain amount of oil, thereby improving its UV absorption.
[0006] Chinese patent application 202310234537.3 discloses an anti-UV leather material for automotive interior. The leather material is prepared from the following components, measured by weight: 30 to 50 parts of water-based epoxy resin; 70 to 80 parts of polyurethane acrylate; 5 to 15 parts of nano-silica; 1 to 2 parts of antioxidant; 1 to 2 parts of retanning agent; 0.11 to 0.22 parts of light stabilizer, wherein the light stabilizer is a composition of phenyl o-hydroxybenzoate, 2,4-dihydroxybenzophenone, and 6-tert-butyl-p-cresol, wherein the phenyl o-hydroxybenzoate is 0.05 to 0.1 parts; 2,4-dihydroxybenzophenone is 0.05 to 0.1 parts; and 6-tert-butyl-p-cresol is 0.01 to 0.02 parts. In this scheme, water-based epoxy resin, polyurethane acrylate and nano-silica are prepared by a blending method to obtain modified leather. The leather material can be endowed with stronger ultraviolet absorption ability, so that the prepared leather has anti-ultraviolet properties. In addition, the scheme points out that polyurethane acrylate is used as a radiation-curing material with good properties, and is used in a synergistic combination with phenyl o-hydroxybenzoate, 2,4-dihydroxybenzophenone and 6-tert-butyl-p-cresol. The use can absorb ultraviolet rays well, and the combined use is better than ordinary anti-ultraviolet agents.
[0007] The problem to be solved by this scheme is: how to develop an anti-ultraviolet artificial leather surface treatment agent which is different from the prior art and has good anti-ultraviolet ability. Summary of the invention
[0008] The purpose of the present invention is to provide an anti-ultraviolet artificial leather surface treatment agent, wherein the ultraviolet absorber in the anti-ultraviolet artificial leather surface treatment agent is mainly used to absorb ultraviolet rays, reduce the damage of ultraviolet rays to leather, thereby prolonging the service life of the leather and alleviating the aging and cracking of the leather, while the free radical scavenger can remove free radicals on the surface of the leather, reduce the oxidation reaction caused by the free radicals, thereby preventing the leather from losing elasticity, cracking and other problems caused by the oxidation reaction on the surface of the leather.
[0009] To achieve the above object, the present application discloses an anti-ultraviolet artificial leather surface treatment agent, comprising an ultraviolet absorber and a free radical scavenger, wherein the ultraviolet absorber is selected from at least one of benzophenone compounds, benzotriazole compounds, and triazine compounds;
[0010] The free radical scavenger is selected from ethylenediaminetetraacetic acid and its derivatives.
[0011] Preferably, the main component of the anti-ultraviolet artificial leather treatment agent is polyester polyol, and the polyester polyol is selected from any one of polyethylene adipate diol, polyethylene adipate diol, polybutylene adipate diol, and polycaprolactone diol.
[0012] Preferably, the following components are included by weight:
[0013]
[0014] Preferably, the diol is selected from at least one of ethylene glycol, propylene glycol, butanediol, pentanediol and hexanediol;
[0015] The diisocyanate is selected from at least one of dicyclohexylmethane diisocyanate, isophorone diisocyanate and xylylene diisocyanate;
[0016] The organic tin catalyst is selected from at least one of dibutyltin dilaurate, dibutyltin dioctoate, and dimethyl distannate.
[0017] Preferably, the following components are included by weight:
[0018]
[0019] Preferably, the benzophenone compound is selected from at least one of 2-hydroxybenzophenone, 4-hydroxybenzophenone and thiobenzophenone;
[0020] The benzotriazole compound is selected from at least one of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2-(2-hydroxy-3,5-di-tert-phenyl)-5-chlorobenzotriazole;
[0021] The triazine compound is selected from at least one of 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, 2-(2-hydroxy-4-hexyloxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-octyloxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(2-hydroxy-4-octyloxyphenyl)-4,6-bis(4-methylbenzene)-1,3,5-triazine;
[0022] The ethylenediaminetetraacetic acid and its derivatives are selected from at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate.
[0023] Preferably, the following components are included by weight:
[0024]
[0025] The ultraviolet absorber is a mixture of benzotriazole compounds and triazine compounds, and the mass ratio of the benzotriazole compounds to the triazine compounds is 1-3:1.
[0026] Preferably, the free radical scavenger is a mixture of ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate, and the mass ratio of ethylenediaminetetraacetic acid to disodium ethylenediaminetetraacetate is 1 to 3:1.
[0027] Preferably, the yellowing resistance grade of the anti-ultraviolet artificial leather surface treatment agent is not less than grade 4.5.
[0028] In addition, the present application also discloses a method for preparing the above-mentioned anti-ultraviolet artificial leather surface treatment agent, wherein an ultraviolet absorber and a free radical scavenger are added to the surface treatment agent and mixed to prepare the anti-ultraviolet artificial leather surface treatment agent.
[0029] The beneficial effects of this application are:
[0030] The present application uses benzophenone compounds, benzotriazole compounds, and triazine compounds as ultraviolet absorbers to effectively absorb ultraviolet rays and reduce the damage of ultraviolet rays to leather; and ethylenediaminetetraacetic acid as a free radical scavenger can remove free radicals, reduce oxidation reactions, and further reduce the oxidative damage caused by ultraviolet rays, thereby enhancing the protective effect of leather, and using free radical scavengers and ultraviolet absorbers at the same time can effectively protect leather and extend its service life. Free radical scavengers can reduce oxidation reactions and prevent leather aging; ultraviolet absorbers can reduce the damage of ultraviolet rays to leather, maintain the color and texture of leather, and thus extend the service life of leather. DETAILED DESCRIPTION
[0031] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0032] Before the examples are presented, the following necessary explanations are first made on the raw materials and preparation methods involved in the examples:
[0033] The raw material information of the embodiment is shown in Table 1:
[0034] Table 1
[0035]
[0036]
[0037] The preparation methods in the embodiments and comparative examples are:
[0038] The polyester polyol, diol, diisocyanate accounting for 30% of the total mass of diisocyanate, organic tin catalyst and solvent are reacted at 95° C. for 6 hours to obtain a prepolymer, then the temperature is lowered to 50° C., the remaining diisocyanate accounting for 70% of the total mass of diisocyanate is added and mixed uniformly to obtain a surface treatment agent, and then the surface treatment agent is stirred and mixed with an ultraviolet absorber and a free radical scavenger to obtain an anti-ultraviolet artificial leather surface treatment agent.
[0039] Examples 1-4
[0040] An anti-ultraviolet artificial leather surface treatment agent, the formula of which is shown in Table 2 by weight:
[0041] Table 2
[0042]
[0043]
[0044] Example 5
[0045] The method is basically the same as Example 1, except that the ultraviolet absorber is prepared by mixing 2-hydroxybenzophenone and 2-(2-hydroxy-5-methylphenyl)benzotriazole, and the mass ratio of the mixture of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2-hydroxybenzophenone is 1:1.
[0046] Example 6
[0047] The method is basically the same as Example 1, except that the ultraviolet absorber is prepared by mixing 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, and the mass ratio of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine is 1:1.
[0048] Example 7
[0049] The method is basically the same as Example 1, except that the ultraviolet absorber is prepared by mixing 2-hydroxybenzophenone and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, and the mass ratio of 2-hydroxybenzophenone and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine is 1:1.
[0050] Example 8
[0051] The method is basically the same as Example 1, except that the free radical scavenger is prepared by mixing ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate, and the mass ratio of ethylenediaminetetraacetic acid to disodium ethylenediaminetetraacetate is 1:1.
[0052] Example 9
[0053] The method is basically the same as Example 1, except that the free radical scavenger is prepared by mixing ethylenediaminetetraacetic acid and tetrasodium ethylenediaminetetraacetate, and the mass ratio of ethylenediaminetetraacetic acid to tetrasodium ethylenediaminetetraacetate is 1:1.
[0054] Example 10
[0055] The method is substantially the same as Example 1, except that the same mass of polybutylene adipate diol is used to replace polyethylene adipate diol.
[0056] Embodiment 11
[0057] The process is substantially the same as Example 1, except that the same mass of isophorone diisocyanate is used to replace dicyclohexylmethane diisocyanate.
[0058] Example 12
[0059] The method is basically the same as Example 1, except that the ultraviolet absorber is prepared by mixing 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, and the mass ratio of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine is 2:1.
[0060] Example 13
[0061] The method is basically the same as Example 1, except that the ultraviolet absorber is prepared by mixing 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, and the mass ratio of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine is 3:1.
[0062] Embodiment 14
[0063] The method is basically the same as Example 1, except that the free radical scavenger is prepared by mixing ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate, and the mass ratio of ethylenediaminetetraacetic acid to disodium ethylenediaminetetraacetate is 2:1.
[0064] Embodiment 15
[0065] The method is basically the same as Example 1, except that the free radical scavenger is prepared by mixing ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate, and the mass ratio of ethylenediaminetetraacetic acid to disodium ethylenediaminetetraacetate is 3:1.
[0066] Comparative Examples 1-7
[0067] A surface treatment agent, the formula of which is shown in Table 3:
[0068] Table 3
[0069]
[0070]
[0071] Performance Testing:
[0072] 1. Yellowing resistance test:
[0073] With reference to QB / T4672-2014, the anti-ultraviolet artificial leather surface treatment agent prepared in each embodiment and comparative example was applied to the surface of white leather purchased from the same batch, and the yellowing resistance of artificial leather and synthetic leather was measured after drying;
[0074] The method for measuring the yellowing resistance of the above-mentioned artificial leather and synthetic leather is:
[0075] UV lamp method
[0076] 1. Cover the radial ends of the sample by 20 mm with a shading sheet, place the sample on the sample tray, with the irradiated surface of the sample facing the light source, and the radial direction of the sample perpendicular to the radial direction of the lamp tube. The surface of the sample is parallel to the bottom of the lamp tube, and the vertical distance is (250 ± 2) mm.
[0077] 2. Start the switch and irradiate the sample under the UV light continuously for an integral multiple of 6 hours. When the specified time (300 hours) is reached, immediately remove the sample from the test chamber and remove the light shielding sheet;
[0078] 3. Test results and evaluation
[0079] The samples are tested in accordance with the provisions of GB / T 2918-1998 under a standard environment of temperature (23±2)℃ and relative humidity (50±10)% in a quasi-multi-light source color matching box using a gray colorimetric card to visually test the color change levels of the covered and uncovered parts of the samples. The color change level is taken as the yellowing level and the result with the largest difference is taken as the final result.
[0080] Tensile strength aging rate after 300 hours of ultraviolet irradiation = (tensile strength after 300 hours of ultraviolet irradiation - initial tensile strength)
[0081] The test results of the embodiments and comparative examples are shown in Table 4:
[0082] Table 4
[0083]
[0084]
[0085] Result analysis:
[0086] 1. Referring to Table 4, it can be seen from Examples 1-4 that, when the total mass fraction remains unchanged, after a small adjustment is made to the addition amount of each component, although the initial tensile strength, the tensile strength after 300 hours of ultraviolet irradiation, and the aging rate of the tensile strength after 300 hours of ultraviolet irradiation of Examples 1-4 fluctuate to a certain extent, the fluctuation range is small;
[0087] 2. It can be seen from Examples 1 and 5-7 that when the ultraviolet absorber is prepared by mixing 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, and the mass ratio of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine is 1:1, the yellowing resistance grade of Example 6 does not change significantly compared with Examples 1, 5, and 7, but the initial tensile strength and tensile strength after 300 hours of ultraviolet irradiation of Example 6 are significantly different. The tensile strength aging rate after ultraviolet irradiation for 300 hours is improved to a certain extent. On the one hand, it can be seen that when the ultraviolet absorber is prepared by mixing 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, the leather treated with this anti-ultraviolet artificial leather surface treatment agent has good anti-ultraviolet aging ability. On the other hand, it can be seen that the leather surface treatment agent using this ultraviolet absorber has more excellent initial tensile strength. It can be seen that the selection of ultraviolet absorbers can also improve the mechanical properties of the surface treatment agent to a certain extent.
[0088] 3. It can be seen from Examples 1 and 8-9 that when the free radical scavenger is prepared by mixing ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate, the tensile strength aging rate after 300 hours of ultraviolet irradiation is significantly lower than that of Examples 1 and 9. It can be seen that no matter whether the free radical scavenger is made of ethylenediaminetetraacetic acid, tetrasodium ethylenediaminetetraacetate or ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, or tetrasodium ethylenediaminetetraacetate, it is impossible to obtain good anti-ultraviolet aging ability similar to that of Example 8;
[0089] 4. It can be seen from Examples 1 and 10-11 that when other polyester polyols and diisocyanates are used to replace polyethylene adipate diol and dicyclohexylmethane diisocyanate in Example 1, the anti-ultraviolet aging ability of Example 10 is improved. It can be seen that polybutylene adipate diol performs better in this application, and this application is more suitable for the preparation of polybutylene adipate diol as a surface treatment agent for polyester polyols, while Example 11 shows weaker anti-ultraviolet aging ability than Example 10;
[0090] 5. It can be seen from Examples 1 and 12-15 that when the mass ratio of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine is 2:1, and the mass ratio of ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate is 2:1, Examples 12 and 14 have better anti-ultraviolet aging ability. It can be seen that the optimization of the addition amount of each component in the ultraviolet absorber and the free radical scavenger also has a crucial influence on the improvement of the anti-ultraviolet aging ability;
[0091] 6. It can be seen from Example 1 and Comparative Examples 1-2 that when the surface treatment agent lacks an ultraviolet absorber or a free radical scavenger, the yellowing resistance of the leather using a surfactant has a significant downward trend, and the anti-ultraviolet aging ability of the leather has a significant decline;
[0092] Further observation of comparative examples 4-6 shows that when the amount of ultraviolet absorber and free radical scavenger added is too small, the yellowing resistance of the leather has a significant downward trend, and the resistance to ultraviolet aging of the leather is significantly reduced; and when the amount of ultraviolet absorber and free radical scavenger added is too much, the resistance to ultraviolet aging of the leather is significantly reduced. It is speculated that the reason for this phenomenon may be that too much ultraviolet absorber and free radical scavenger have a negative impact on the leather material, destroying the original structure and properties of the leather under long-term attachment, causing the leather to lose elasticity, become fragile, and reduce its resistance to ultraviolet aging.
Claims
1. An anti-ultraviolet artificial leather surface treatment agent, characterized in that, Contains an ultraviolet absorber and a free radical scavenger, wherein the ultraviolet absorber is selected from at least one of benzophenone compounds, benzotriazole compounds, and triazine compounds; The free radical scavenger is selected from ethylenediaminetetraacetic acid and its derivatives.
2. The anti-ultraviolet artificial leather surface treating agent according to claim 1, characterized in that The main component of the anti-ultraviolet artificial leather treatment agent is polyester polyol, and the polyester polyol is selected from any one of polyethylene adipate glycol, polyethylene adipate glycol propylene glycol, polybutylene adipate glycol, and polycaprolactone glycol.
3. The anti-ultraviolet artificial leather surface treating agent according to claim 1, characterized in that, By mass, it includes the following components:
4. The anti-ultraviolet artificial leather surface treating agent according to claim 3, characterized in that: The diol is selected from at least one of ethylene glycol, propylene glycol, butanediol, pentanediol and hexanediol; The diisocyanate is selected from at least one of dicyclohexylmethane diisocyanate, isophorone diisocyanate and xylylene diisocyanate; The organic tin catalyst is selected from at least one of dibutyltin dilaurate, dibutyltin dioctoate, and dimethyl distannate.
5. The anti-ultraviolet artificial leather surface treating agent according to claim 1, characterized in that: By mass, it includes the following components:
6. The anti-ultraviolet artificial leather surface treating agent according to claim 1, characterized in that: The benzophenone compound is selected from at least one of 2-hydroxybenzophenone, 4-hydroxybenzophenone and thiobenzophenone; The benzotriazole compound is selected from at least one of 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2-(2-hydroxy-3,5-di-tert-phenyl)-5-chlorobenzotriazole; The triazine compound is selected from at least one of 2,4-bis(2-hydroxy-4-butylphenyl)-6-phenyl-1,3,5-triazine, 2-(2-hydroxy-4-hexyloxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-octyloxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(2-hydroxy-4-octyloxyphenyl)-4,6-bis(4-methylbenzene)-1,3,5-triazine; The ethylenediaminetetraacetic acid and its derivatives are selected from at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate.
7. The anti-ultraviolet artificial leather surface treating agent according to claim 5, characterized in that: By mass, it includes the following components: The ultraviolet absorber is a mixture of benzotriazole compounds and triazine compounds, and the mass ratio of the benzotriazole compounds to the triazine compounds is 1-3:
1.
8. The anti-ultraviolet artificial leather surface treating agent according to claim 7, characterized in that: The free radical scavenger is a mixture of ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate, and the mass ratio of ethylenediaminetetraacetic acid to disodium ethylenediaminetetraacetate is 1 to 3:
1.
9. The anti-ultraviolet artificial leather surface treating agent according to claim 1, characterized in that: The yellowing resistance grade of the anti-ultraviolet artificial leather surface treatment agent is not less than grade 4.
5.
10. A method for preparing the anti-ultraviolet artificial leather surface treatment agent according to claims 1-9, characterized in that: An ultraviolet absorber and a free radical scavenger are added to a surface treatment agent and mixed to prepare an anti-ultraviolet artificial leather surface treatment agent.
Citation Information
Cited By
Preparation method of anti-ultraviolet and anti-infrared dual-protection artificial leather
CN119978771A
Hard polyvinyl chloride film with high weather resistance and low gloss as well as preparation method and application of hard polyvinyl chloride film
CN122127713A