Rubber material for shock pad and preparation method thereof
By introducing modified silicone oil and modified polyurethane into rubber materials to form an interpenetrating polymer network, combined with the dispersion effect of modified graphene, the problems of insufficient oil resistance and weather resistance of existing rubber materials are solved, and better shock absorption performance and durability are achieved.
Patent Information
- Application Number
- CN202411488025.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing rubber materials are insufficient in terms of oil resistance and weather resistance, making it difficult to meet the increasingly demanding requirements for vibration damping.
By adding modified silicone oil and modified polyurethane to rubber materials, the perfluorocyclobutyl groups in the modified silicone oil and the disulfide bonds and hindered urea bonds in the modified polyurethane form an interpenetrating polymer network. Combined with the dispersion effect of modified graphene, the shock absorption performance of the material is improved, and the oil resistance and weather resistance are enhanced through the synergistic effect of modified silicone oil and modified polyurethane.
It significantly improves the shock absorption performance of rubber materials, while also enhancing their oil resistance and weather resistance, and strengthening the friction and dispersion effect between the material's molecular chains.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber materials, and in particular to a rubber material for a shock-absorbing pad and a preparation method thereof. Background Art
[0002] With the improvement of human living standards, human beings have higher and higher requirements for the environment. The development of science, technology and industry has increased the power of machinery and equipment, accelerated the speed, and the hazards of vibration and noise have become more and more prominent. Rubber shock-absorbing pads, as a rubber material with high elasticity and high viscosity, play an obvious role in buffering, shock absorption and dynamic sealing.
[0003] Currently commonly used rubber materials such as natural rubber have good dynamic performance, durability and processing performance, but their oil resistance and weather resistance are poor, and they cannot meet the increasingly high shock absorption requirements. Summary of the invention
[0004] The object of the present invention is to provide a rubber material for a shock-absorbing pad and a preparation method thereof, which solves the problem that the existing rubber material has insufficient oil resistance and weather resistance, and improves its shock-absorbing performance.
[0005] The purpose of the present invention can be achieved by the following technical scheme: A rubber material for a shock-absorbing pad is prepared by the following steps: Step S1: weigh the following raw materials in parts by weight: 50-60 parts of natural rubber, 6-10 parts of modified polyurethane, 12-15 parts of modified silicone oil, 8-10 parts of white carbon black, 2-3 parts of zinc oxide, 0.8-1 part of accelerator, 0.8-1 part of antioxidant, 1-2 parts of bis(2,4-dichlorobenzoyl) peroxide and 1-2 parts of sulfur; Step S2: adding natural rubber, modified polyurethane, modified silicone oil, white carbon black, zinc oxide, accelerator and antioxidant into an internal mixer, mixing for 8 minutes at a speed of 80 rpm and a temperature of 70° C., then adding bis(2,4-dichlorobenzoyl) peroxide and sulfur, thinning through 10 times, and vulcanizing the material, wherein the first stage vulcanization temperature is 150° C. and the vulcanization time is 25 minutes, and the second stage vulcanization temperature is 180° C. and the vulcanization time is 30 minutes, thereby obtaining a rubber material for a shock absorbing pad; The modified silicone oil is prepared by the following steps: Step A1: eugenol, cesium carbonate and dimethyl sulfoxide are mixed, stirred at a stirring rate of 240-300 rpm and room temperature for 12 hours, 1,2-dibromotetrafluoroethane is added, the temperature is raised to 50°C, and the reaction is carried out for 16 hours to obtain intermediate 1, intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane and Custer catalyst are mixed, the temperature is stirred at 600 rpm and 60°C, the reaction is carried out for 12 hours, zinc powder and anhydrous acetonitrile are added, the temperature is raised to 120°C, and the reaction is carried out for 18 hours to obtain intermediate 2; The amount ratio of eugenol, cesium carbonate and 1,2-dibromotetrafluoroethane is 0.1-0.15 mol: 0.15 mol: 0.1-0.15 mol, and the amount ratio of intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane, Custer catalyst and zinc powder is 0.08-0.1 mol: 0.04-0.05 mol: 0.5 mL: 2.5 g; During the reaction, under the action of cesium carbonate, the phenolic hydroxyl group in eugenol reacts with 1,2-dibromotetrafluoroethane to undergo fluoroalkylation reaction to form an ether bond and a 1-bromotetrafluoroethane group, thereby obtaining an intermediate 1. Under the action of a Custer catalyst, a double bond in the intermediate 1 reacts with a silicon-hydrogen bond in 1,1,3,3,5,5-hexamethyltrisiloxane to undergo a silylation reaction, and the intermediate 1 is connected to the 1,1,3,3,5,5-hexamethyltrisiloxane. Zinc powder is then added, and the 1-bromotetrafluoroethane group undergoes a dehalogenation reaction to form a trifluorovinyl group, thereby obtaining an intermediate 2. Step A2: Mix intermediate 1, dodecanethiol, ethyl acetate and acetonitrile, stir and add azobisisobutyronitrile under nitrogen protection at a stirring rate of 240-300 rpm and a temperature of 80°C, react for 12-16 hours, then add zinc powder and heat to 120°C, react for 18 hours to obtain intermediate 3; The ratio of intermediate 1, dodecanethiol, azobisisobutyronitrile and zinc powder is 0.08-0.1 mol: 0.08-0.1 mol: 2 g: 2.5 g; During the reaction, under the action of azobisisobutyronitrile, the double bond in intermediate 1 undergoes a click reaction with the thiol group in dodecanethiol, and then zinc powder is added, and the 1-bromotetrafluoroethane group in intermediate 1 undergoes a dehalogenation reaction to form a trifluorovinyl group, thereby obtaining intermediate 3; Step A3: Mix intermediate 2 and intermediate 3, and react for 9 hours under nitrogen protection, stirring rate of 300-360 rpm, temperature of 175°C, cool to room temperature, add tri(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane and dichloromethane, react for 12 hours, then add methylvinyldimethoxysilane and dimethyldimethoxysilane, raise the temperature to 90°C, and continue to react for 24 hours to obtain modified silicone oil; The amount ratio of intermediate 2, intermediate 3, tris(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane, methylvinyldimethoxysilane and dimethyldimethoxysilane is 0.01-0.02mol: 0.02-0.04mol: 0.05g: 0.01-0.02mol: 0.01mol: 0.08mol; During the reaction, the intermediate 2 undergoes a cyclodimerization reaction with the trifluorovinyl group in the intermediate 3 to form a perfluorocyclobutyl group, which then undergoes a Piers-Rubinsztajn reaction with the methoxy group in the intermediate 2 and the silicon-hydrogen bond in 1,1,3,3-tetramethyldisiloxane under the action of tri(pentafluorophenyl)borane to form a silicon-oxygen bond, and then methylvinyldimethoxysilane and dimethyldimethoxysilane are added to obtain a modified silicone oil containing a double bond; The modified polyurethane is prepared by the following steps: Step B1: Carboxyl functionalized graphene and N,N-dimethylformamide were mixed and ultrasonically dispersed for 1 hour, and isophorone diisocyanate and dibutyltin dilaurate were added at a stirring rate of 600 rpm and a temperature of 85° C. The mixture was reacted for 24 hours to obtain modified graphene; The amount ratio of carboxyl functionalized graphene, isophorone diisocyanate and dibutyltin dilaurate is 0.1g:0.02-0.03mol:0.5mL; During the reaction, under the action of dibutyltin dilaurate catalyst, the isocyanate group in isophorone diisocyanate reacts with the carboxyl group in carboxyl functionalized graphene to obtain modified graphene containing isocyanate groups. Step B2: Mix cystamine dihydrochloride and deionized water, stir at a rate of 200-240 rpm, add potassium hydroxide solution, and react for 15-20 min to obtain cystamine; mix cystamine and diethyl maleate, stir at a rate of 200-240 rpm, and react for 24 h at 80° C. to obtain intermediate a; The molar concentration of potassium hydroxide solution is 10 mol / L, the dosage ratio of cystamine dihydrochloride and potassium hydroxide solution is 18-20 g: 25-30 mL, and the dosage ratio of cystamine and diethyl maleate is 0.1 mol: 0.1-0.11 mol; During the reaction, cystamine dihydrochloride reacts with potassium hydroxide solution to obtain cystamine, and the primary amine group at the middle end of cystamine reacts with the double bond in diethyl maleate to produce intermediate a; Step B3: Modified graphene, intermediate a, commercially available PCL2000 polycaprolactone diol, isophorone diisocyanate and dibutyltin diosilicate were mixed, and the mixture was reacted for 6-8 hours at a stirring rate of 500-600 rpm and a temperature of 60° C., and 2-hydroxyethyl acrylate was added, and the reaction was continued for 3 hours to obtain modified polyurethane; The amount ratio of modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate, dibutyltin diosilicate and 2-hydroxyethyl acrylate is 0.2-0.3g: 0.01mol: 20-25g: 0.02mol: 0.05g: 0.02mol; During the reaction, the isocyanate groups in the modified graphene and isophorone diisocyanate react with the secondary amine groups in the intermediate a and the hydroxyl groups in the polycaprolactone diol, and then 2-hydroxyethyl acrylate is added for end-capping to obtain a modified polyurethane; Beneficial effects of the invention: The invention relates to a rubber material for a shock-absorbing pad and a preparation method thereof. By adding modified silicone oil and modified polyurethane to the rubber material, during the vulcanization process of the rubber material, natural rubber forms a cross-linked network under the action of sulfur. Since both the modified silicone oil and the modified polyurethane contain double bonds, a cross-linked network can also be formed under the action of bis(2,4-dichlorobenzoyl) peroxide at the temperature of the second-stage vulcanization, thereby forming an interpenetrating polymer network, thereby improving the shock-absorbing performance of the rubber material. Since the modified silicone oil contains a silicone oil segment containing perfluorocyclobutyl and the modified polyurethane is added at the same time, the oil resistance of the rubber material can be improved to a certain extent. and weather resistance, and because the modified polyurethane contains disulfide bonds and hindered urea bonds, the hindered urea bonds can form multiple hydrogen bonds. When subjected to external forces, the multiple hydrogen bonds and disulfide bonds are broken preferentially, thereby improving the shock absorbing performance of the rubber material, and because there are long chains of dodecanethiol in the modified silicone oil and multiple hydrogen bonds in the modified polyurethane, they can play a synergistic role, thereby increasing the friction between the molecular chains, thereby improving the shock absorbing performance of the rubber material, and the modified polyurethane is based on carboxylated graphene, and the carboxyl functionalized graphene is modified first to improve the dispersion of the carboxyl functionalized graphene in the rubber material, thereby improving the shock absorbing performance of the rubber material. DETAILED DESCRIPTION
[0006] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0007] A rubber material for a shock-absorbing pad is prepared by the following steps: Step S1: weigh the following raw materials in parts by weight: 50 parts of commercially available SCR5 natural rubber, 6 parts of modified polyurethane, 12 parts of modified silicone oil, 8 parts of commercially available A200 white carbon black, 2 parts of zinc oxide, 0.8 parts of commercially available CZ accelerator, 0.8 parts of commercially available 4020 antioxidant, 1 part of bis(2,4-dichlorobenzoyl) peroxide, and 1 part of sulfur; Step S2: adding natural rubber, modified polyurethane, modified silicone oil, white carbon black, zinc oxide, accelerator and antioxidant into an internal mixer, mixing for 8 minutes at a speed of 80 rpm and a temperature of 70° C., then adding bis(2,4-dichlorobenzoyl) peroxide and sulfur, thinning through 10 times, and vulcanizing the material, wherein the first stage vulcanization temperature is 150° C. and the vulcanization time is 25 minutes, and the second stage vulcanization temperature is 180° C. and the vulcanization time is 30 minutes, thereby obtaining a rubber material for a shock absorbing pad; The modified silicone oil is prepared by the following steps: Step A1: eugenol, cesium carbonate and dimethyl sulfoxide are mixed, stirred at a stirring rate of 240 rpm and room temperature for 12 hours, 1,2-dibromotetrafluoroethane is added, the temperature is raised to 50°C, and the reaction is carried out for 16 hours to obtain intermediate 1, intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane and Custer catalyst are mixed, the temperature is stirred at 600 rpm and 60°C, the reaction is carried out for 12 hours, zinc powder and anhydrous acetonitrile are added, the temperature is raised to 120°C, and the reaction is carried out for 18 hours to obtain intermediate 2; The amount ratio of eugenol, cesium carbonate and 1,2-dibromotetrafluoroethane is 0.1 mol: 0.15 mol: 0.1 mol, and the amount ratio of intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane, Custer catalyst and zinc powder is 0.08 mol: 0.04 mol: 0.5 mL: 2.5 g; Step A2: Intermediate 1, dodecanethiol, ethyl acetate and acetonitrile were mixed, and azobisisobutyronitrile was added under nitrogen protection at a stirring rate of 240 rpm and a temperature of 80°C, and the mixture was reacted for 16 hours. Zinc powder was then added and the mixture was heated to 120°C and reacted for 18 hours to obtain intermediate 3; The ratio of intermediate 1, dodecanethiol, azobisisobutyronitrile and zinc powder is 0.08 mol: 0.08 mol: 2 g: 2.5 g; Step A3: Intermediate 2 and intermediate 3 were mixed, and the mixture was reacted for 9 hours under nitrogen protection, stirring at a rate of 300 rpm and a temperature of 175°C. The mixture was cooled to room temperature and tri(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane and dichloromethane were added, and the mixture was reacted for 12 hours. Methylvinyldimethoxysilane and dimethyldimethoxysilane were then added and the mixture was heated to 90°C. The mixture was reacted for 24 hours to obtain a modified silicone oil. The amount ratio of intermediate 2, intermediate 3, tris(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane, methylvinyldimethoxysilane and dimethyldimethoxysilane is 0.01mol: 0.02mol: 0.05g: 0.01mol: 0.01mol: 0.08mol; The modified polyurethane is prepared by the following steps: Step B1: commercially available Xianfeng carboxyl functionalized graphene and N,N-dimethylformamide were mixed and ultrasonically dispersed for 1 hour, and isophorone diisocyanate and dibutyltin dilaurate were added at a stirring rate of 600 rpm and a temperature of 85°C, and reacted for 24 hours to obtain modified graphene; The amount ratio of carboxyl functionalized graphene, isophorone diisocyanate and dibutyltin dilaurate was 0.1 g: 0.02 mol: 0.5 mL; Step B2: Cystamine dihydrochloride and deionized water are mixed, stirred at a stirring rate of 200 rpm and room temperature, and potassium hydroxide solution is added to react for 20 minutes to obtain cystamine; cystamine and diethyl maleate are mixed, stirred at a stirring rate of 200 rpm and a temperature of 80° C., and reacted for 24 hours to obtain intermediate a; The molar concentration of potassium hydroxide solution is 10 mol / L, the amount ratio of cystamine dihydrochloride and potassium hydroxide solution is 18 g:25 mL, and the amount ratio of cystamine and diethyl maleate is 0.1 mol:0.1 mol; Step B3: the modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate and dibutyltin diosilicate were mixed, and the mixture was reacted for 8 hours at a stirring rate of 500 rpm and a temperature of 60° C., and 2-hydroxyethyl acrylate was added, and the reaction was continued for 3 hours to obtain a modified polyurethane; The amount ratio of modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate, dibutyltin diosilicate and 2-hydroxyethyl acrylate is 0.2g:0.01mol:20g:0.02mol:0.05g:0.02mol. Example 2
[0008] A rubber material for a shock-absorbing pad is prepared by the following steps: Step S1: weigh the following raw materials in parts by weight: 60 parts of commercially available SCR5 natural rubber, 6 parts of modified polyurethane, 12 parts of modified silicone oil, 10 parts of commercially available A200 white carbon black, 3 parts of zinc oxide, 1 part of commercially available CZ accelerator, 1 part of commercially available 4020 antioxidant, 2 parts of bis(2,4-dichlorobenzoyl) peroxide and 2 parts of sulfur; Step S2: adding natural rubber, modified polyurethane, modified silicone oil, white carbon black, zinc oxide, accelerator and antioxidant into an internal mixer, mixing for 8 minutes at a speed of 80 rpm and a temperature of 70° C., then adding bis(2,4-dichlorobenzoyl) peroxide and sulfur, thinning through 10 times, and vulcanizing the material, wherein the first stage vulcanization temperature is 150° C. and the vulcanization time is 25 minutes, and the second stage vulcanization temperature is 180° C. and the vulcanization time is 30 minutes, thereby obtaining a rubber material for a shock absorbing pad; The modified silicone oil is prepared by the following steps: Step A1: eugenol, cesium carbonate and dimethyl sulfoxide are mixed, stirred at a stirring rate of 300 rpm and room temperature for 12 hours, 1,2-dibromotetrafluoroethane is added, the temperature is raised to 50°C, and the reaction is carried out for 16 hours to obtain intermediate 1, intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane and Custer catalyst are mixed, the temperature is stirred at 600 rpm and 60°C, the reaction is carried out for 12 hours, zinc powder and anhydrous acetonitrile are added, the temperature is raised to 120°C, and the reaction is carried out for 18 hours to obtain intermediate 2; The amount ratio of eugenol, cesium carbonate and 1,2-dibromotetrafluoroethane is 0.15 mol: 0.15 mol: 0.15 mol, and the amount ratio of intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane, Custer catalyst and zinc powder is 0.08 mol: 0.05 mol: 0.5 mL: 2.5 g; Step A2: Intermediate 1, dodecanethiol, ethyl acetate and acetonitrile were mixed, and azobisisobutyronitrile was added under nitrogen protection at a stirring rate of 300 rpm and a temperature of 80°C, and the mixture was reacted for 12 hours, and then zinc powder was added and the mixture was heated to 120°C and reacted for 18 hours to obtain intermediate 3; The ratio of intermediate 1, dodecanethiol, azobisisobutyronitrile and zinc powder is 0.08 mol: 0.1 mol: 2 g: 2.5 g; Step A3: Intermediate 2 and intermediate 3 were mixed, and the mixture was reacted for 9 hours under nitrogen protection, stirring at a rate of 360 rpm and a temperature of 175°C. The mixture was cooled to room temperature and tri(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane and dichloromethane were added, and the mixture was reacted for 12 hours. Methylvinyldimethoxysilane and dimethyldimethoxysilane were then added and the mixture was heated to 90°C. The mixture was reacted for 24 hours to obtain a modified silicone oil. The amount ratio of intermediate 2, intermediate 3, tris(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane, methylvinyldimethoxysilane and dimethyldimethoxysilane is 0.02mol: 0.03mol: 0.05g: 0.02mol: 0.01mol: 0.08mol; The modified polyurethane is prepared by the following steps: Step B1: commercially available Xianfeng carboxyl functionalized graphene and N,N-dimethylformamide were mixed and ultrasonically dispersed for 1 hour, and isophorone diisocyanate and dibutyltin dilaurate were added at a stirring rate of 600 rpm and a temperature of 85°C, and reacted for 24 hours to obtain modified graphene; The amount ratio of carboxyl functionalized graphene, isophorone diisocyanate and dibutyltin dilaurate was 0.1 g: 0.03 mol: 0.5 mL; Step B2: Cystamine dihydrochloride and deionized water are mixed, stirred at a stirring rate of 240 rpm and room temperature, and potassium hydroxide solution is added to react for 15 minutes to obtain cystamine; cystamine and diethyl maleate are mixed, stirred at a stirring rate of 240 rpm and a temperature of 80° C., and reacted for 24 hours to obtain intermediate a; The molar concentration of potassium hydroxide solution is 10 mol / L, the amount ratio of cystamine dihydrochloride and potassium hydroxide solution is 20 g:25 mL, and the amount ratio of cystamine and diethyl maleate is 0.1 mol:0.1 mol; Step B3: the modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate and dibutyltin diosilicate were mixed, and the mixture was reacted for 6 hours at a stirring rate of 600 rpm and a temperature of 60° C., and 2-hydroxyethyl acrylate was added, and the reaction was continued for 3 hours to obtain a modified polyurethane; The amount ratio of modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate, dibutyltin diosilicate and 2-hydroxyethyl acrylate is 0.2g:0.01mol:25g:0.02mol:0.05g:0.02mol. Example 3
[0009] A rubber material for a shock-absorbing pad is prepared by the following steps: Step S1: weigh the following raw materials in parts by weight: 60 parts of commercially available SCR5 natural rubber, 10 parts of modified polyurethane, 15 parts of modified silicone oil, 10 parts of commercially available A200 white carbon black, 3 parts of zinc oxide, 1 part of commercially available CZ accelerator, 1 part of commercially available 4020 antioxidant, 2 parts of bis(2,4-dichlorobenzoyl) peroxide and 2 parts of sulfur; Step S2: adding natural rubber, modified polyurethane, modified silicone oil, white carbon black, zinc oxide, accelerator and antioxidant into an internal mixer, mixing for 8 minutes at a speed of 80 rpm and a temperature of 70° C., then adding bis(2,4-dichlorobenzoyl) peroxide and sulfur, thinning through 10 times, and vulcanizing the material, wherein the first stage vulcanization temperature is 150° C. and the vulcanization time is 25 minutes, and the second stage vulcanization temperature is 180° C. and the vulcanization time is 30 minutes, thereby obtaining a rubber material for a shock absorbing pad; The modified silicone oil is prepared by the following steps: Step A1: eugenol, cesium carbonate and dimethyl sulfoxide are mixed, stirred at a stirring rate of 300 rpm and room temperature for 12 hours, 1,2-dibromotetrafluoroethane is added, the temperature is raised to 50°C, and the reaction is carried out for 16 hours to obtain intermediate 1, intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane and Custer catalyst are mixed, the temperature is stirred at 600 rpm and 60°C, the reaction is carried out for 12 hours, zinc powder and anhydrous acetonitrile are added, the temperature is raised to 120°C, and the reaction is carried out for 18 hours to obtain intermediate 2; The amount ratio of eugenol, cesium carbonate and 1,2-dibromotetrafluoroethane is 0.15 mol: 0.15 mol: 0.15 mol, and the amount ratio of intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane, Custer catalyst and zinc powder is 0.1 mol: 0.05 mol: 0.5 mL: 2.5 g; Step A2: Intermediate 1, dodecanethiol, ethyl acetate and acetonitrile were mixed, and azobisisobutyronitrile was added under nitrogen protection, stirring at a rate of 300 rpm and a temperature of 80°C, and the mixture was reacted for 16 hours. Zinc powder was then added and the mixture was heated to 120°C and reacted for 18 hours to obtain intermediate 3; The ratio of intermediate 1, dodecanethiol, azobisisobutyronitrile and zinc powder is 0.1 mol: 0.1 mol: 2 g: 2.5 g; Step A3: Intermediate 2 and intermediate 3 were mixed, and the mixture was reacted for 9 hours under nitrogen protection, stirring at a rate of 360 rpm and a temperature of 175°C. The mixture was cooled to room temperature and tri(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane and dichloromethane were added, and the mixture was reacted for 12 hours. Methylvinyldimethoxysilane and dimethyldimethoxysilane were then added and the mixture was heated to 90°C. The mixture was reacted for 24 hours to obtain a modified silicone oil. The amount ratio of intermediate 2, intermediate 3, tris(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane, methylvinyldimethoxysilane and dimethyldimethoxysilane is 0.02mol: 0.04mol: 0.05g: 0.02mol: 0.01mol: 0.08mol; The modified polyurethane is prepared by the following steps: Step B1: commercially available Xianfeng carboxyl functionalized graphene and N,N-dimethylformamide were mixed and ultrasonically dispersed for 1 hour, and isophorone diisocyanate and dibutyltin dilaurate were added at a stirring rate of 600 rpm and a temperature of 85°C, and reacted for 24 hours to obtain modified graphene; The amount ratio of carboxyl functionalized graphene, isophorone diisocyanate and dibutyltin dilaurate was 0.1 g: 0.03 mol: 0.5 mL; Step B2: Cystamine dihydrochloride and deionized water are mixed, stirred at a stirring rate of 240 rpm and room temperature, and potassium hydroxide solution is added for reaction for 20 minutes to obtain cystamine; cystamine and diethyl maleate are mixed, stirred at a stirring rate of 240 rpm and a temperature of 80° C., and the reaction is carried out for 24 hours to obtain intermediate a; The molar concentration of potassium hydroxide solution is 10 mol / L, the amount ratio of cystamine dihydrochloride and potassium hydroxide solution is 20 g:30 mL, and the amount ratio of cystamine and diethyl maleate is 0.1 mol:0.11 mol; Step B3: the modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate and dibutyltin disilicate were mixed, and the mixture was reacted for 8 hours at a stirring rate of 600 rpm and a temperature of 60° C., and 2-hydroxyethyl acrylate was added, and the reaction was continued for 3 hours to obtain a modified polyurethane; The amount ratio of modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate, dibutyltin diosilicate and 2-hydroxyethyl acrylate is 0.3g:0.01mol:25g:0.02mol:0.05g:0.02mol.
[0010] Comparative Example 1 Compared with Example 3, this comparative example is characterized in that dodecanethiol in the preparation process of the modified silicone oil in Example 3 is replaced by ethyl mercaptan, and the other steps are the same.
[0011] Comparative Example 2 Compared with Example 3, this comparative example replaces 1,2-dibromotetrafluoroethane with bromoethane in the preparation process of the modified silicone oil in Example 3, and the other steps are the same.
[0012] Comparative Example 3 Compared with Example 3, this comparative example replaces the modified graphene in the preparation process of the modified polyurethane in Example 3 with commercially available Xianfeng carboxyl functionalized graphene, and the other steps are the same.
[0013] Comparative Example 4 Compared with Example 3, this comparative example is characterized in that the intermediate a in the preparation process of the modified polyurethane in Example 3 is replaced with 1,4-butanediamine, and the other steps are the same.
[0014] Comparative Example 5 Compared with Example 3, the second-stage vulcanization process in the preparation process of the rubber material for the shock-absorbing pad in Example 3 is removed, and the other steps are the same.
[0015] Take the rubber materials for shock absorbing pads prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Example 5, and test their tensile strength and elongation at break with reference to GB / T 528-2009, at a tensile speed of 500 mm / min, and test their compression permanent deformation with reference to GB / T 1683-2018, under the test conditions of 70°C×24h, and measure their dynamic and static stiffness ratio with reference to GB / T 9870.1-2006, with a sample size of 5 cm×5 cm×2 cm, and apply a cyclic load stress of 0-360 N at a dynamic rate of compression rate of 5 mm / min, repeat three times to obtain the static stiffness, and then at a compression frequency of 10 Hz, under the conditions of a periodic load of 200-750 N, continuously compress the sample 1000 times to obtain the dynamic stiffness, and calculate the dynamic and static stiffness ratio, with reference to GB / T 3512-2014, the sample was subjected to hot air aging, the aging condition was 150℃×72h, and the oil resistance test was performed on it with reference to GB / T1690-2010, the oil resistance condition was 150℃×72h, IRM903 oil, the test results are as follows: Test items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Tensile strength (MPa) 29.5 29.6 29.9 29.7 28.4 25.2 26.3 21.7 Compression set (%) 29.2 28.9 28.7 29.1 30.4 31.4 32.5 34.5 Dynamic-static stiffness ratio 1.34 1.37 1.38 1.30 1.26 1.23 1.18 1.08 Tensile strength after heat aging (MPa) 28.0 28.3 28.5 28.3 25.0 23.8 24.9 18.5 Tensile strength after oil resistance test (MPa) 23.7 23.9 24.1 24.0 20.7 20.1 21.1 14.1 It can be seen from the test results in the table shown that when Example 1, Example 2 and Example 3 are compared with Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5, Comparative Example 1 replaces dodecanethiol with ethyl mercaptan in the preparation process of the modified silicone oil in Example 3, and its shock absorption performance decreases to a certain extent, indicating that dodecanethiol can improve the shock absorption performance of the rubber material. Comparative Example 2 replaces 1,2-dibromotetrafluoroethane with bromoethane in the preparation process of the modified silicone oil in Example 3, and its heat resistance and oil resistance decrease significantly, indicating that the presence of perfluorocyclobutyl groups can effectively improve the heat resistance and oil resistance of rubber materials. Comparative Example 3 replaces the modified graphite in the preparation process of the modified polyurethane in Example 3. In comparative example 4, intermediate a in the preparation process of the modified polyurethane in Example 3 was replaced by 1,4-butanediamine, and its shock absorbing performance was significantly reduced, indicating that the presence of disulfide bonds and hindered urea bonds can effectively improve the shock absorbing performance of the rubber material. In comparative example 5, the two-stage vulcanization process in the preparation process of the rubber material for the shock-absorbing pad in Example 3 was removed. Due to the lack of the two-stage vulcanization, the double bonds in the modified silicone oil and the modified polyurethane cannot be cross-linked, and various properties of the rubber material are significantly reduced.
[0016] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0017] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a rubber material for a shock-absorbing pad, characterized in that: The method is as follows: Step S1: Weigh the following raw materials in parts by weight: 50-60 parts of natural rubber, 6-10 parts of modified polyurethane, 12-15 parts of modified silicone oil, 8-10 parts of white carbon black, 2-3 parts of zinc oxide, 0.8-1 parts of accelerator, 0.8-1 parts of antioxidant, 1-2 parts of bis(2,4-dichlorobenzoyl) peroxide and 1-2 parts of sulfur; Step S2: adding natural rubber, modified polyurethane, modified silicone oil, white carbon black, zinc oxide, accelerator and antioxidant into an internal mixer, mixing for 8 minutes at a speed of 80 rpm and a temperature of 70° C., then adding bis(2,4-dichlorobenzoyl) peroxide and sulfur, thinning through 10 times, and vulcanizing the material, wherein the first stage vulcanization temperature is 150° C. and the vulcanization time is 25 minutes, and the second stage vulcanization temperature is 180° C. and the vulcanization time is 30 minutes, thereby obtaining a rubber material for a shock absorbing pad; The modified silicone oil is prepared by the following steps: Step A1: eugenol, cesium carbonate and dimethyl sulfoxide are mixed, stirred at a stirring rate of 240-300 rpm and room temperature for 12 hours, 1,2-dibromotetrafluoroethane is added, the temperature is raised to 50°C, and the reaction is carried out for 16 hours to obtain intermediate 1, intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane and Custer catalyst are mixed, the temperature is stirred at 600 rpm and 60°C, the reaction is carried out for 12 hours, zinc powder and anhydrous acetonitrile are added, the temperature is raised to 120°C, and the reaction is carried out for 18 hours to obtain intermediate 2; Step A2: Mix intermediate 1, dodecanethiol, ethyl acetate and acetonitrile, stir and add azobisisobutyronitrile under nitrogen protection at a stirring rate of 240-300 rpm and a temperature of 80°C, react for 12-16 hours, then add zinc powder and heat to 120°C, react for 18 hours to obtain intermediate 3; Step A3: Mix intermediate 2 and intermediate 3, and react for 9 hours under nitrogen protection, stirring rate of 300-360 rpm, temperature of 175°C, cool to room temperature, add tri(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane and dichloromethane, react for 12 hours, then add methylvinyldimethoxysilane and dimethyldimethoxysilane, raise the temperature to 90°C, and continue to react for 24 hours to obtain modified silicone oil; The modified polyurethane is prepared by the following steps: Step B1: Carboxyl functionalized graphene and N,N-dimethylformamide were mixed and ultrasonically dispersed for 1 hour, and isophorone diisocyanate and dibutyltin dilaurate were added at a stirring rate of 600 rpm and a temperature of 85° C. The mixture was reacted for 24 hours to obtain modified graphene; Step B2: Mix cystamine dihydrochloride and deionized water, stir at a rate of 200-240 rpm, add potassium hydroxide solution, and react for 15-20 min to obtain cystamine; mix cystamine and diethyl maleate, stir at a rate of 200-240 rpm, and react for 24 h at 80° C. to obtain intermediate a; Step B3: Mix the modified graphene, intermediate a, commercially available PCL2000 polycaprolactone diol, isophorone diisocyanate and dibutyltin disilicate, react for 6-8 hours at a stirring rate of 500-600 rpm and a temperature of 60°C, then add 2-hydroxyethyl acrylate and continue the reaction for 3 hours to obtain a modified polyurethane.
2. The method for preparing a rubber material for a shock-absorbing pad according to claim 1, characterized in that: In step A1: the usage ratio of eugenol, cesium carbonate and 1,2-dibromotetrafluoroethane is 0.1-0.15 mol: 0.15 mol: 0.1-0.15 mol, and the usage ratio of intermediate 1, 1,1,3,3,5,5-hexamethyltrisiloxane, Custer catalyst and zinc powder is 0.08-0.1 mol: 0.04-0.05 mol: 0.5 mL: 2.5 g.
3. The method for preparing a rubber material for a shock-absorbing pad according to claim 1, characterized in that: In step A2, the ratio of the intermediate 1, dodecanethiol, azobisisobutyronitrile and zinc powder is 0.08-0.1 mol: 0.08-0.1 mol: 2 g: 2.5 g.
4. The method for preparing a rubber material for a shock-absorbing pad according to claim 1, characterized in that: In step A3: the usage ratio of intermediate 2, intermediate 3, tris(pentafluorophenyl)boron, 1,1,3,3-tetramethyldisiloxane, methylvinyldimethoxysilane and dimethyldimethoxysilane is 0.01-0.02 mol: 0.02-0.04 mol: 0.05 g: 0.01-0.02 mol: 0.01 mol: 0.08 mol.
5. The method for preparing a rubber material for a shock-absorbing pad according to claim 1, characterized in that: In step B1: the amount ratio of carboxyl functionalized graphene, isophorone diisocyanate and dibutyltin dilaurate is 0.1 g: 0.02-0.03 mol: 0.5 mL.
6. The method for preparing a rubber material for a shock-absorbing pad according to claim 1, characterized in that: In step B2, the molar concentration of the potassium hydroxide solution is 10 mol / L, the amount ratio of cystamine dihydrochloride to the potassium hydroxide solution is 18-20 g: 25-30 mL, and the amount ratio of cystamine to diethyl maleate is 0.1 mol: 0.1-0.11 mol.
7. The method for preparing a rubber material for a shock-absorbing pad according to claim 1, characterized in that: In step B3: the amount ratio of modified graphene, intermediate a, polycaprolactone diol, isophorone diisocyanate, dibutyltin diosilicate and 2-hydroxyethyl acrylate is 0.2-0.3g:0.01mol:20-25g:0.02mol:0.05g:0.02mol.
8. A rubber material for a shock-absorbing pad, characterized in that: Prepared according to any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of high-temperature-resistant elastomer
CN115894768A
Rubber shock pad and preparation process thereof
CN116731408A
Cited By
High-performance solvent-free blade wear-resistant self-repairing finish paint and preparation method thereof
CN120795761A
A high-performance solvent-free blade wear-resistant self-healing topcoat and its preparation method
CN120795761B