Skin-touch 3D printing consumable and preparation method thereof

Through the synergistic effect of components such as polyurethane elastomer, modified silica and silane coupling agent, the contradiction between tactile simulation and mechanical properties in 3D printing materials is solved, and efficient 3D printing performance and long-term stability are achieved. In the fields of medical care and education, the application of bionic materials has been promoted.

CN118994881APending Publication Date: 2024-11-22GUANGDONG BIYING ZENGCAI MANUFACTURING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411109157.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing 3D printing materials are difficult to maintain good mechanical and 3D printing performance while achieving high-simulation skin touch, and there are problems such as high cost, complex methods and insufficient environmental friendliness.

Method used

Using polyurethane elastomer, modified silica, polyethylene glycol and silane coupling agent, skin-skin-skin-skin-skin-skin-coupling agent and other components, the skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin-skin Ensure thermal stability.

Benefits of technology

It achieves high-simulation skin touch, excellent mechanical properties and excellent 3D printing performance, while reducing production costs and method complexity, meeting environmentally friendly requirements, and is suitable for medical and education fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of 3D printing consumables, in particular to a skin-touch 3D printing consumable material and a preparation method of the skin-touch 3D printing consumable material. 15 to 25 parts of modified silicon dioxide; 10 to 15 parts of polyethylene glycol, wherein the molecular weight of the polyethylene glycol is 4000; 1-3 parts of a silane coupling agent; through the synergistic effect of the modified silicon dioxide, the polyurethane elastomer and the polyethylene glycol, the extremely high skin touch simulation degree is achieved, and the touch score is as high as 8.7. The modified silicon dioxide simulates the microstructure of the skin on the nanoscale, the polyethylene glycol provides proper lubrication feeling, the polyurethane elastomer endows the whole material with flexibility, and the material disclosed by the invention shows perfect combination of high strength (the tensile strength reaches 28.1 MPa) and high flexibility (the elongation at break is 480%).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing consumables, and in particular to a skin-feeling 3D printing consumable material and a preparation method thereof. Background Art

[0002] 3D printing technology has developed rapidly in various fields in recent years, among which the application of bionic materials is particularly eye-catching. Especially in the fields of medical care, education and product design, there is a growing demand for 3D printing materials with a touch similar to human skin. However, existing technologies face many challenges in achieving high-simulation skin touch while maintaining good 3D printing performance and mechanical properties:

[0003] 1. Insufficient touch simulation: Existing 3D printing materials are mainly thermoplastics (such as PLA, ABS). Although these materials have good formability, they feel stiff and are far from the softness and texture of human skin. Although some flexible materials (such as TPU) have improved in softness, they still cannot accurately simulate the complex touch of skin.

[0004] 2. The contradiction between mechanical properties and softness: In order to improve the degree of tactile simulation, researchers try to use softer materials or increase the content of plasticizers. However, this often leads to a significant decrease in the mechanical strength and durability of the material, which cannot meet the needs of practical applications. Especially in the fields of medical models and training supplies, the material needs to have both skin-like touch and sufficient mechanical strength. This contradiction is difficult to resolve with existing technologies.

[0005] 3. Poor 3D printing performance: Many materials with soft touch have serious problems in the 3D printing process. For example, poor material fluidity leads to low printing accuracy, weak interlayer bonding causes easy delamination of printed products, and poor thermal stability causes deformation during printing. These problems seriously limit the application of bionic materials in the field of 3D printing.

[0006] 4. Poor long-term stability: Some materials that improve the touch by adding plasticizers or surface treatment often face the problem of performance degradation during long-term use. For example, plasticizer migration causes the material to harden, and the surface treatment layer falls off, causing the touch to change. This makes it impossible for the product to maintain stable performance during use.

[0007] 5. Cost and method complexity: In order to solve the above problems, some researchers have tried to use complex multi-material printing technology or post-processing methods. However, these methods often greatly increase the production cost and method complexity, which is not conducive to large-scale application.

[0008] 6. Insufficient environmental friendliness: Some existing bionic materials use environmentally unfriendly chemical additives or difficult-to-degrade polymers to achieve specific properties, which is contrary to the requirements of sustainable development.

[0009] In view of the above problems, it is particularly necessary to develop a material that can simultaneously achieve high-simulation skin touch, excellent mechanical properties and outstanding 3D printing performance. This will not only promote the application of bionic materials in the field of 3D printing, but will also bring revolutionary progress to medical models, education and training, personalized products and other fields. Summary of the invention

[0010] In view of the above problems, it is of great practical significance and urgent need to develop a skin-feeling 3D printing consumable and a preparation method thereof that can solve these technical problems at the same time.

[0011] The present invention discloses a skin-feeling 3D printing consumable, which comprises the following components in parts by weight:

[0012] Polyurethane elastomer 60-70 parts;

[0013] 15-25 parts of modified silicon dioxide;

[0014] 10-15 parts of polyethylene glycol, wherein the molecular weight of the polyethylene glycol is 4000;

[0015] 1-3 parts of silane coupling agent;

[0016] Antioxidant 0.1-0.5 parts.

[0017] Specifically, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0018] Specifically, the antioxidant is BHT.

[0019] The method for preparing the skin-feeling 3D printing consumables comprises the following steps:

[0020] a) melting the polyurethane elastomer at 180-200° C.;

[0021] b) adding modified silicon dioxide to the molten polyurethane elastomer and stirring evenly;

[0022] c) adding polyethylene glycol to the mixture obtained in step b) and continuing stirring;

[0023] d) adding a silane coupling agent and an antioxidant to the mixture obtained in step c), and stirring for 30-60 minutes;

[0024] e) cooling the mixture obtained in step d) to room temperature and cutting into pellets;

[0025] f) using a single screw extruder to extrude the granules obtained in step e) into filaments, and then winding them into a bobbin after cooling.

[0026] Specifically, in step b), the modified silicon dioxide is added slowly.

[0027] Specifically, in step a), the melting temperature of the polyurethane elastomer is 190°C.

[0028] Specifically, in step d), the stirring time is 45 minutes.

[0029] Specifically, the method further comprises drying the particles obtained in step e) before step f).

[0030] Specifically, the drying process is carried out at a temperature of 60-80° C. and for a time of 2-4 hours.

[0031] The present invention also discloses skin-feeling 3D printing consumables obtained by the preparation method.

[0032] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0033] 1. Excellent skin simulation: Through the synergistic effect of modified silica, polyurethane elastomer and polyethylene glycol, the present invention achieves extremely high skin touch simulation (touch score up to 8.7 points). Modified silica simulates the microstructure of the skin at the nanoscale, polyethylene glycol provides an appropriate lubricity, and polyurethane elastomer gives the material overall flexibility.

[0034] 2. Excellent mechanical properties: The material of the present invention exhibits a perfect combination of high strength (tensile strength of 28.1 MPa) and high flexibility (elongation at break of 480%). This is due to the enhanced network structure formed by the modified silica and the enhanced interfacial bonding force of the silane coupling agent. This unique structure enables the material to have sufficient mechanical strength and durability while maintaining a soft touch.

[0035] 3. Excellent 3D printing performance: The material of the present invention exhibits extremely high printing accuracy (dimensional accuracy deviation is only 0.12%) and excellent surface quality (surface roughness Ra value is 2.5μm). The addition of polyethylene glycol improves the fluidity of the material, while the network structure of modified silica improves the dimensional stability of the material. The presence of silane coupling agent reduces the defects of the interlayer interface and significantly improves the printing quality and interlayer bonding strength.

[0036] 4. Excellent interfacial bonding strength: The peel strength of the material of the present invention is as high as 4.8N / mm, far exceeding that of the comparative example. This strong interfacial bonding strength originates from the chemical bond formed by the silane coupling agent between the modified silica surface and the polyurethane matrix, which not only improves the overall strength of the material, but also significantly improves the interlayer bonding strength of the 3D printed product.

[0037] 5. Excellent thermal stability: Through the thermal stabilization effect of modified silica, the plasticizing effect of polyethylene glycol and the synergistic effect of the antioxidant BHT, the material of the present invention exhibits excellent thermal stability. This not only ensures the stability of the 3D printing process, but also ensures that the printed product can maintain good performance in long-term use.

[0038] 6. Simple and efficient preparation method: The present invention adopts a simple melt mixing method, which does not require a complicated post-processing method, greatly reduces the production cost and method complexity, and is conducive to large-scale application.

[0039] 7. Environmental friendliness: All components used in the present invention have good biocompatibility and environmental friendliness, and meet the requirements of sustainable development.

[0040] In summary, the present invention successfully solves the contradiction between tactile simulation and mechanical properties in 3D printing materials through the synergistic effect of multiple components, and achieves excellent printing performance and long-term stability. This innovative material design opens up new possibilities for bionic materials and functional 3D printing, and is expected to bring revolutionary applications in the fields of medical models, simulation training, personalized products, etc., and promote the development of 3D printing technology to a higher level. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] A skin-feeling 3D printing consumable, the consumable comprising the following components in parts by weight:

[0044] Components (parts by weight):

[0045] Polyurethane elastomer:60

[0046] Modified silica: 15

[0047] Polyethylene glycol (molecular weight 4000): 10

[0048] γ-Aminopropyltriethoxysilane:1

[0049] BHT:0.1

[0050] The preparation method comprises the following steps:

[0051] 1. Melt 60 parts of polyurethane elastomer at 180°C for 30 minutes;

[0052] 2. Slowly add 15 parts of modified silica to the molten polyurethane at a rate of 1 g / min, stirring at a speed of 200 rpm, and stir for 60 minutes until uniform;

[0053] 3. Add 10 parts of polyethylene glycol (molecular weight 4000) and continue stirring at 200 rpm for 30 minutes;

[0054] 4. Add 1 part of γ-aminopropyltriethoxysilane and 0.1 part of BHT and stir at 250 rpm for 30 minutes;

[0055] 5. Cool the mixture to room temperature and use a granulator to cut into pellets with a particle size of 3 mm;

[0056] 6. Dry at 60°C for 2 hours;

[0057] 7. Use a single screw extruder (screw diameter 25 mm, L / D ratio 20:1) to extrude the granules into filaments with a diameter of 1.75 mm at 190°C, and wind them into a bobbin after cooling.

[0058] Example 2

[0059] A skin-feeling 3D printing consumable, the consumable comprising the following components in parts by weight:

[0060] Polyurethane elastomer:70

[0061] Modified silica: 25

[0062] Polyethylene glycol (molecular weight 4000): 15

[0063] γ-Aminopropyltriethoxysilane:3

[0064] BHT:0.5

[0065] The preparation method comprises the following steps:

[0066] 1. Melt 70 parts of polyurethane elastomer at 200°C for 45 minutes;

[0067] 2. Slowly add 25 parts of modified silica to the molten polyurethane at a rate of 2 g / min, stirring at a speed of 300 rpm, and stir for 90 minutes until uniform;

[0068] 3. Add 15 parts of polyethylene glycol (molecular weight 4000) and continue stirring at 300 rpm for 45 minutes;

[0069] 4. Add 3 parts of γ-aminopropyltriethoxysilane and 0.5 parts of BHT and stir at 350 rpm for 60 minutes;

[0070] 5. Cool the mixture to room temperature and use a granulator to cut into pellets with a particle size of 5 mm;

[0071] 6. Dry at 80°C for 4 hours;

[0072] 7. Use a single screw extruder (screw diameter 30mm, L / D ratio 25:1) to extrude the granules into filaments with a diameter of 2.85mm at 210℃, and wind them into a bobbin after cooling.

[0073] Example 3

[0074] A skin-feeling 3D printing consumable, the consumable comprising the following components in parts by weight:

[0075] Polyurethane elastomer:65

[0076] Modified silica: 20

[0077] Polyethylene glycol (molecular weight 4000): 12

[0078] γ-Aminopropyltriethoxysilane:2

[0079] BHT: 0.3

[0080] Preparation method:

[0081] 1. Melt 65 parts of polyurethane elastomer at 190°C for 40 minutes;

[0082] 2. Slowly add 20 parts of modified silica to the molten polyurethane at a rate of 1.5 g / min, stirring at a speed of 250 rpm, and stir for 75 minutes until uniform;

[0083] 3. Add 12 parts of polyethylene glycol (molecular weight 4000) and continue stirring at 250 rpm for 40 minutes;

[0084] 4. Add 2 parts of γ-aminopropyltriethoxysilane and 0.3 parts of BHT and stir at 300 rpm for 45 minutes;

[0085] 5. Cool the mixture to room temperature and use a granulator to cut into pellets with a particle size of 4 mm;

[0086] 6. Dry at 70°C for 3 hours;

[0087] 7. Use a single screw extruder (screw diameter 28 mm, L / D ratio 22:1) to extrude the granules into filaments with a diameter of 2.00 mm at 200°C, and wind them into a bobbin after cooling.

[0088] Example 4

[0089] A skin-feeling 3D printing consumable, the consumable comprising the following components in parts by weight:

[0090] Polyurethane elastomer:68

[0091] Modified silica:22

[0092] Polyethylene glycol (molecular weight 4000): 13

[0093] γ-Aminopropyltriethoxysilane:2.5

[0094] BHT:0.4

[0095] The preparation method comprises the following steps:

[0096] 1. Melt 68 parts of polyurethane elastomer at 195°C for 35 minutes;

[0097] 2. Slowly add 22 parts of modified silica to the molten polyurethane at a rate of 1.8 g / min, stirring at a speed of 275 rpm, and stir for 80 minutes until uniform;

[0098] 3. Add 13 parts of polyethylene glycol (molecular weight 4000) and continue stirring at 275 rpm for 35 minutes;

[0099] 4. Add 2.5 parts of γ-aminopropyltriethoxysilane and 0.4 parts of BHT and stir at 325 rpm for 50 minutes;

[0100] 5. Cool the mixture to room temperature and use a granulator to cut into pellets with a particle size of 4.5 mm;

[0101] 6. Dry at 75°C for 3.5 hours;

[0102] 7. Use a single screw extruder (screw diameter 29 mm, L / D ratio 23:1) to extrude the granules into filaments with a diameter of 2.50 mm at 205°C, and wind them into a bobbin after cooling.

[0103] Comparative Example 1 (corresponding to Example 1, lacking modified silicon dioxide):

[0104] Components (parts by weight):

[0105] Polyurethane elastomer:60

[0106] Polyethylene glycol (molecular weight 4000): 10

[0107] γ-Aminopropyltriethoxysilane:1

[0108] BHT:0.1

[0109] Preparation method:

[0110] 1. Melt 60 parts of polyurethane elastomer at 180°C for 30 minutes;

[0111] 2. Add 10 parts of polyethylene glycol (molecular weight 4000) and stir at 200 rpm for 30 minutes;

[0112] 3. Add 1 part of γ-aminopropyltriethoxysilane and 0.1 part of BHT and stir at 250 rpm for 30 minutes;

[0113] 4. The subsequent steps are the same as those in Example 1.

[0114] Comparative Example 2 (corresponding to Example 2, replacing the modified silicon dioxide with ordinary silicon dioxide):

[0115] Components (parts by weight):

[0116] Polyurethane elastomer:70

[0117] Ordinary silica: 25

[0118] Polyethylene glycol (molecular weight 4000): 15

[0119] γ-Aminopropyltriethoxysilane:3

[0120] BHT:0.5

[0121] Preparation method:

[0122] Same as Example 2, but ordinary silica is used instead of modified silica in step 2. Comparative Example 3 (corresponding to Example 3, changing the molecular weight of polyethylene glycol):

[0123] Components (parts by weight):

[0124] Polyurethane elastomer:65

[0125] Modified silica: 20

[0126] Polyethylene glycol (molecular weight 2000): 12

[0127] γ-Aminopropyltriethoxysilane:2

[0128] BHT: 0.3

[0129] Preparation method:

[0130] Same as Example 3, but using polyethylene glycol with a molecular weight of 2000.

[0131] Comparative Example 4 (corresponding to Example 4, lacking a silane coupling agent):

[0132] Components (parts by weight):

[0133] Polyurethane elastomer:68

[0134] Modified silica:22

[0135] Polyethylene glycol (molecular weight 4000): 13

[0136] BHT:0.4

[0137] Preparation method:

[0138] Same as Example 4, but omitting the step of adding γ-aminopropyltriethoxysilane.

[0139] Comparative Example 5 (corresponding to Example 1, changing the component contents):

[0140] Components (parts by weight):

[0141] Polyurethane elastomer:50

[0142] Modified silica: 35

[0143] Polyethylene glycol (molecular weight 4000): 20

[0144] γ-Aminopropyltriethoxysilane:1

[0145] BHT:0.1

[0146] Preparation method:

[0147] 1. Melt 50 parts of polyurethane elastomer at 180°C for 30 minutes;

[0148] 2. Slowly add 35 parts of modified silica to the molten polyurethane at a rate of 1 g / min, stirring at a speed of 200 rpm, and stir for 90 minutes until uniform;

[0149] 3. Add 20 parts of polyethylene glycol (molecular weight 4000) and continue stirring at 200 rpm for 45 minutes;

[0150] 4. The subsequent steps are the same as those in Example 1.

[0151] Comparative Example 6 (corresponding to Example 2, changing the preparation temperature):

[0152] Components (parts by weight):

[0153] Same as Example 2

[0154] Preparation method:

[0155] 1. Melt 70 parts of polyurethane elastomer at 160°C for 45 minutes;

[0156] 2. Slowly add 25 parts of modified silica to the molten polyurethane at a rate of 2 g / min, stirring at a speed of 300 rpm, and stir for 90 minutes until uniform;

[0157] 3. Add 15 parts of polyethylene glycol (molecular weight 4000) and continue stirring at 300 rpm for 45 minutes;

[0158] 4. Add 3 parts of γ-aminopropyltriethoxysilane and 0.5 parts of BHT and stir at 350 rpm for 60 minutes;

[0159] 5. Cool the mixture to room temperature and use a granulator to cut into pellets with a particle size of 5 mm;

[0160] 6. Dry at 80°C for 4 hours;

[0161] 7. Use a single screw extruder (screw diameter 30 mm, L / D ratio 25:1) to extrude the granules into filaments with a diameter of 2.85 mm at 180°C, and wind them into a bobbin after cooling.

[0162] These six comparative examples respectively verify the importance of modified silica (Comparative Examples 1 and 2), the influence of polyethylene glycol molecular weight (Comparative Example 3), the role of silane coupling agent (Comparative Example 4), the importance of component content (Comparative Example 5) and the influence of preparation temperature (Comparative Example 6). Through these comparative examples, the importance of each key component and method parameter of the present invention can be fully verified, highlighting the creativity and superiority of the present invention.

[0163] According to the mechanism of action of the present invention, we designed the following test model to evaluate the effectiveness of the solution:

[0164] 1. Skin touch simulation test

[0165] 2. Mechanical properties test

[0166] 3.3D printing performance evaluation

[0167] 4. Microstructure Analysis

[0168] 5. Interface bonding strength test

[0169] The following are the detailed experimental conditions, method steps and results of each test model:

[0170] 1. Skin touch simulation test

[0171] Experimental conditions: room temperature 25℃, relative humidity 50%

[0172] Experimental methods:

[0173] a) Use a 3D printer to print a sample plate of 10cm×10cm×0.5cm

[0174] b) Invite 20 volunteers to conduct blind touch test and scoring

[0175] c) Rating standard: 1-10 points, 1 is the least like skin, 10 is the most like skin

[0176] d) Calculate the average score

[0177] 2. Mechanical properties test

[0178] Experimental conditions: room temperature 25℃, relative humidity 50%

[0179] Experimental methods:

[0180] a) Prepare dumbbell-shaped samples according to ASTM D638

[0181] b) Use a universal testing machine to test tensile strength and elongation at break

[0182] c) Test each group of samples 5 times and take the average value

[0183] 3.3D printing performance evaluation experimental conditions: printing temperature 210℃, printing speed 60mm / s, layer thickness 0.2mm Experimental method:

[0184] a) Print standard test model (25mm cube)

[0185] b) Measurement dimensional accuracy (deviation from design dimensions)

[0186] c) Evaluate surface quality (using a surface roughness tester)

[0187] d) Each group of samples was tested 3 times and the average value was taken

[0188] 4. Microstructure Analysis

[0189] Experimental conditions: room temperature 25℃

[0190] Experimental methods:

[0191] a) Observation of sample cross section using field emission scanning electron microscopy (FE-SEM) b) Acceleration voltage 10 kV, magnification 5000×

[0192] c) Observe and record the dispersion of silica and the interface bonding conditions 5. Interface bonding strength test

[0193] Experimental conditions: room temperature 25℃, relative humidity 50%

[0194] Experimental methods:

[0195] a) Prepare dumbbell-shaped samples and pre-form cracks in the middle

[0196] b) Peel test using a universal testing machine

[0197] c) Measurement of peel strength

[0198] d) Test each group of samples 5 times and take the average value

[0199] The test results are shown in the following table:

[0200] Table 1: Skin touch simulation test and mechanical properties test results

[0201] sample Touch rating Tensile strength(MPa) Elongation at break (%) Example 1 8.2 25.3 450 Example 2 8.7 28.1 480 Example 3 8.5 26.8 465 Example 4 8.6 27.5 475 Comparative Example 1 6.1 18.2 320 Comparative Example 2 7.3 22.6 385 Comparative Example 3 7.8 24.5 430 Comparative Example 4 7.5 23.8 410 Comparative Example 5 6.8 20.4 350 Comparative Example 6 8 25.9 455

[0202] Table 2: 3D printing performance evaluation and interface bonding test results

[0203] sample Dimensional accuracy deviation (%) Surface roughness (Ra, μm) Peel strength (N / mm) Example 1 0.15 2.8 4.2 Example 2 0.12 2.5 4.8 Example 3 0.14 2.6 4.5 Example 4 0.13 2.5 4.7 Comparative Example 1 0.28 4.2 2.6 Comparative Example 2 0.22 3.5 3.4 Comparative Example 3 0.18 3.1 3.9 Comparative Example 4 0.2 3.3 3.2 Comparative Example 5 0.25 3.8 3 Comparative Example 6 0.16 2.9 4.3

[0204] Microstructure analysis results:

[0205] The SEM images of Examples 1-4 show that the modified silica is evenly dispersed in the polyurethane matrix, and the particle size is in the range of 50-100 nm. A clear network structure is observed, indicating that there is good interface bonding between the silica and the polyurethane matrix. The SEM images of Comparative Examples 1-6 show poor dispersibility and interface bonding, especially Comparative Examples 1 and 2.

[0206] According to the comprehensive test results, Example 2 performed best, reaching optimal levels in terms of skin touch, mechanical properties, 3D printing performance and interface bonding strength.

[0207] The present invention has the following unexpected technical effects:

[0208] 1. Ultra-high skin simulation: The touch score of Example 2 reached 8.7 points, far exceeding that of traditional 3D printing materials. This is because the modified silica simulates the microstructure of the skin at the nanoscale, while the polyethylene glycol provides an appropriate lubrication. The addition of the silane coupling agent further enhances the synergy between the components, forming a unique network structure, so that the material maintains sufficient strength while presenting a soft touch similar to skin.

[0209] 2. Excellent balance between mechanical properties and flexibility: Example 2 exhibits a tensile strength of 28.1 MPa and an elongation at break of 480%. This combination of high strength and high flexibility is extremely rare in 3D printing materials. This is due to the enhanced network structure formed by modified silica and the characteristics of the polyurethane elastomer itself. The addition of silane coupling agent significantly enhances the interface bonding between the filler and the matrix, allowing the material to effectively transfer stress when subjected to external force.

[0210] 3. Excellent 3D printing performance: The dimensional accuracy deviation of Example 2 is only 0.12%, and the surface roughness Ra value is 2.5μm, which are much better than ordinary 3D printing materials. This is because the addition of polyethylene glycol improves the fluidity of the material, and the network structure of modified silica improves the dimensional stability of the material. The presence of silane coupling agent reduces the defects of the interlayer interface, thereby improving the printing quality.

[0211] 4. Strong interfacial bonding: The peel strength of Example 2 reached 4.8 N / mm, which is much higher than that of the comparative example. This strong interfacial bonding comes from the chemical bond formed by the silane coupling agent between the modified silica surface and the polyurethane matrix. This not only improves the overall strength of the material, but also significantly improves the interlayer bonding of the 3D printed product and reduces the risk of delamination.

[0212] 5. Synergistic thermal stability: Although not directly reflected in the above test, it can be inferred from the results of Comparative Example 6 that the formula of the present invention has excellent thermal stability. This is due to the thermal stabilization effect of modified silica, the plasticizing effect of polyethylene glycol, and the synergistic effect of the antioxidant BHT. This thermal stability is not only beneficial to the 3D printing process, but also ensures that the printed product maintains good performance during use.

[0213] The present invention successfully solves the contradiction between tactile simulation and mechanical properties in 3D printing materials through the synergistic effect of multiple components, while achieving excellent printing performance. This unique formula design opens up new possibilities for bionic materials and functional 3D printing, and is expected to bring revolutionary applications in the fields of medical models, simulation training, personalized products, etc.

[0214] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A skin-feeling 3D printing consumable, characterized in that , the consumables include the following components in parts by weight: Polyurethane elastomer 60-70 parts; 15-25 parts of modified silicon dioxide; 10-15 parts of polyethylene glycol, wherein the molecular weight of the polyethylene glycol is 4000; 1-3 parts of silane coupling agent; Antioxidant 0.1-0.5 parts.

2. The skin-feeling 3D printing consumable according to claim 1, characterized in that , the silane coupling agent is γ-aminopropyltriethoxysilane.

3. The skin-feeling 3D printing consumable according to claim 1, characterized in that , the antioxidant is BHT.

4. The method for preparing the skin-feeling 3D printing consumables according to any one of claims 1 to 3, characterized in that , including the following steps: a) melting the polyurethane elastomer at 180-200° C.; b) adding modified silicon dioxide to the molten polyurethane elastomer and stirring evenly; c) adding polyethylene glycol to the mixture obtained in step b) and continuing stirring; d) adding a silane coupling agent and an antioxidant to the mixture obtained in step c), and stirring for 30-60 minutes; e) cooling the mixture obtained in step d) to room temperature and cutting into pellets; f) using a single screw extruder to extrude the granules obtained in step e) into filaments, and then winding them into a bobbin after cooling.

5. The preparation method according to claim 4, characterized in that In step b), the modified silicon dioxide is added slowly.

6. The preparation method according to claim 4, characterized in that In step a), the melting temperature of the polyurethane elastomer is 190°C.

7. The preparation method according to claim 4, characterized in that , in step d), the stirring time is 45 minutes.

8. The preparation method according to claim 4, characterized in that , further comprising drying the particles obtained in step e) before step f).

9. The preparation method according to claim 8, characterized in that The drying temperature is 60-80°C and the drying time is 2-4 hours.

10. A skin-feeling 3D printing consumables prepared according to the preparation method according to any one of claims 4 to 9.