Silicone rubber material for high-temperature-resistant and fatigue-resistant steering protective sleeve and preparation method of silicone rubber material
By using modified gas-phase white carbon black, strong-wire powder and heat-resistant agent in silicon rubber materials, combined with specific vulcanization processes, the service life of silicon rubber under high temperature and fatigue conditions is solved, and high strength is achieved , silicone rubber material with excellent heat resistance and dynamic performance.
Patent Information
- Application Number
- CN202310564028.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-22
AI Technical Summary
The existing silicone rubber materials have a short service life under high temperature and fatigue conditions, making it difficult to meet the application needs of high temperature and dynamic motion.
The modified gas-phase method of white carbon black, Qiangwei powder, WACK H0 heat resistance agent and metal oxide heat resistance agent are used to improve the high temperature and fatigue resistance of silicone rubber through specific vulcanization processes and formulation optimization.
It significantly improves the tensile strength, tear-break elongation and high-temperature aging resistance of silicone rubber, extends its service life, can work stably at 200℃ high temperature, and reciprocate at 125℃ high temperature for 2 months without cracks.
Smart Images

Figure BDA0004236123070000101 
Figure BDA0004236123070000111 
Figure BDA0004236123070000112
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber materials, and in particular to a silicone rubber material for a high-temperature-resistant and fatigue-resistant steering protective sleeve and a preparation method thereof. Background Art
[0002] The solid silicone rubber commonly used in the market is methyl vinyl silicone rubber (MVQ), which is made by introducing a small amount of vinyl units (generally 0.03%-0.3% molar fraction) into the side chain of dimethyl silicone rubber. Although phenyl silicone rubber has higher heat resistance than dimethyl silicone rubber, its price is about 10 times that of MVQ, so it is not used much. The conventional operating temperature of conventional dimethyl silicone rubber is 175°C, and its service life can be evaluated by tensile strength or elongation at break (according to the national standard GB / T 20028-2005, Arrhenius is used to calculate the maximum operating temperature and service life of vulcanized rubber).
[0003] For example, products such as protective sleeves close to the engine, protective sleeves on temperature sensor thermocouples, steering protective sleeves, etc. have high operating temperatures and certain reciprocating motions, and complex operating conditions, which put forward high requirements on the performance of silicone rubber products. Therefore, it is very necessary to develop a silicone rubber formula with high temperature resistance, excellent dynamic performance and long service life, which is of great significance to broaden the application of silicone rubber under high heat resistance dynamic conditions. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a silicone rubber material for a high temperature and fatigue resistant steering protective sleeve and a preparation method thereof.
[0005] The present invention provides a high temperature and fatigue resistant silicone rubber material for a steering protective sleeve, comprising the following raw materials in parts by weight: 50-60 parts of MVQ raw rubber, 20-40 parts of modified fumed silica, 5-30 parts of Qiangwei powder, 1-8 parts of a structure control agent, 0.5-1.5 parts of a vulcanizing agent, 0.5-2 parts of a Wacker H0 heat resistant agent, 0.5-2.5 parts of a metal oxide heat resistant agent, and 0.3-1 parts of a black masterbatch;
[0006] The modified fumed silica is obtained by surface-modifying fumed silica with a mercaptosilane coupling agent, wherein the BET value of the fumed silica is 200-400 m 2 / g; preferably, the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:2-100:8. The modification mechanism is that the silane coupling agent can inhibit the interaction between siloxane and hydroxyl groups on the surface of silica, and link silica to rubber through chemical bonds. At the same time, the unsaturated mercapto group can improve the coupling efficiency and enhance the reinforcement of silica.
[0007] In the present invention, the mass fraction of MVQ raw rubber can be 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, and 60 parts; the mass fraction of fumed silica can be 20.0 parts, 21.0 parts, 22.0 parts, 23.0 parts, 24.0 parts, 25.0 parts, 26.0 parts, 27.0 parts, 28.0 parts, 29.0 parts, 30.0 parts, 31.0 parts, 32.0 parts, 33.0 parts, 34.0 parts, 35. 0 parts, 36.0 parts, 37.0 parts, 38.0 parts, 39.0 parts, 40.0 parts; the mass parts of Qiangwei powder can be 5.0 parts, 6.0 parts, 7.0 parts, 8.0 parts, 9.0 parts, 10.0 parts, 11.0 parts, 12.0 parts, 13.0 parts, 14.0 parts, 15.0 parts, 16.0 parts, 17.0 parts, 18.0 parts, 19.0 parts, 20.0 parts, 21.0 parts, 22.0 parts, 23.0 parts, 24.0 parts, 25.0 parts, 26.0 parts , 27.0 parts, 28.0 parts, 29.0 parts, 30.0 parts; the mass fraction of the structure control agent can be 1.0 parts, 1.5 parts, 2.0 parts, 2.5 parts, 3.0 parts, 3.5 parts, 4.0 parts, 4.5 parts, 5.0 parts, 5.5 parts, 6.0 parts, 6.5 parts, 7.0 parts, 7.5 parts, 8.0 parts; the mass fraction of the vulcanizing agent can be 0.5 parts, 0.6 parts, 0.70 parts, 0.80 parts, 0.90 parts, 1.00 parts, 1.10 parts, 1.20 parts, The mass fractions of Wacker H0 heat resisting agent can be 0.5 parts, 0.7 parts, 1.0 parts, 1.2 parts, 1.5 parts, 2 parts; the mass fractions of metal oxide heat resisting agent can be 0.5 parts, 0.7 parts, 1.0 parts, 1.1 parts, 1.3 parts, 1.5 parts, 2 parts, 2.5 parts; the mass fractions of black master paste can be 0.3 parts, 0.4 parts, 0.5 parts, 0.60 parts, 0.70 parts, 0.80 parts, 0.90 parts, 1.0 parts.
[0008] Preferably, the MVQ raw rubber is methyl vinyl silicone rubber 110. By selecting MVQ raw rubber with a suitable vinyl content, the vulcanization degree of the MVQ raw rubber can be significantly improved under the premise of having a certain high temperature resistance, so that the cross-linking network of the vulcanized rubber is more perfect and uniform, and the obtained silicone rubber material has the excellent properties of high strength, high temperature resistance, excellent dynamic performance and long life.
[0009] Preferably, the relative molecular weight of the methyl vinyl silicone rubber 110 is 60-80×10 4 , the vinyl content is 0.03-0.1%. A higher molecular weight can ensure that the material has a higher tensile strength, and the appropriate vinyl content can ensure both a certain vulcanization bond and appropriate high temperature resistance, ensuring the high temperature performance requirements of the protective cover material.
[0010] Preferably, the preparation method of the modified fumed silica is: atomizing the mercaptosilane coupling agent through a pressurizing device and then evenly spraying it into the fumed silica, and reacting at 120-140° C. for 1-3 hours to obtain the modified fumed silica.
[0011] Preferably, the fumed silica is fumed silica with a BET value of 200-400 m 2 / g. Since fumed silica has a higher structural degree than precipitated silica, it is more active and has better reinforcement for silicone rubber.
[0012] Preferably, the Qiangwei powder is a vinyl silane-modified Qiangwei powder, which can play a synergistic role with fumed silica. The vinyl contained in the Qiangwei powder can participate in the vulcanization reaction, improve the compatibility with silicone rubber and thus improve the reinforcement effect.
[0013] Preferably, the structure control agent is D4 (octamethylcyclotetrasiloxane), which is added as an inert intermediate of synthetic silicone rubber to reduce the physical cross-linking effect between silicone rubbers and reduce the increase in hardness.
[0014] Preferably, the vulcanizing agent is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (abbreviated as di-2,5), 4,4-di(tert-butylperoxy) valerate n-butyl ester (trade name 230XL) or a combination thereof.
[0015] Preferably, the metal oxide heat resistant agent is nano-sized cerium oxide, red iron oxide or a combination thereof. In the present invention, by adding Wacker HO heat resistant agent and metal oxide heat resistant agent with high thermal conductivity in a suitable proportion, the thermal conductivity of the rubber material can be improved, and the free radicals generated during the aging process of silicone rubber can be eliminated, thereby playing a synergistic role and improving the high temperature aging resistance of the silicone rubber material.
[0016] A method for preparing the high temperature and fatigue resistant silicone rubber material for a steering protective sleeve comprises the following steps:
[0017] S1. Prepare materials by mass, and mix MVQ raw rubber, structure control agent, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, metal oxide heat resistant agent, and black masterbatch to obtain a premixed rubber;
[0018] S2, first add the vulcanizing agent to the premixed rubber for secondary mixing, and then perform a vulcanization in the mold to obtain a primary vulcanized rubber;
[0019] S3, subjecting the primary vulcanized rubber to secondary vulcanization to obtain.
[0020] Preferably, in S1, the primary mixing temperature is 110-130°C, the rotation speed is 20-50 r / min, and the time is 3-8 h.
[0021] Preferably, in S2, the temperature of the secondary mixing is 0-40°C, the speed is 20-50r / min, and the time is 5-30min; in S3, the temperature of the primary vulcanization is 160-180°C, the time is 160-320s, and the pressure is 140-180Kgf / cm 2 .
[0022] Preferably, in S3, the temperature of the secondary vulcanization is 180-200° C. and the time is 2-4 hours.
[0023] A high temperature and fatigue resistant silicone rubber material for a steering protective sleeve is prepared by the preparation method.
[0024] The beneficial effects of the present invention are as follows:
[0025] The formula of the present invention treats fumed silica by using a suitable surface treatment agent and process, thereby ensuring uniform dispersion and interaction of the silica in the silicone rubber matrix, and by synergizing with the vinyl-modified strong powder, improving the tensile strength and elongation at break, thereby improving fatigue resistance and service life; by using a suitable low-temperature mixing process, the defect of the mixed rubber becoming soft when heated is avoided, and the shear force is improved, so that the reinforcing agent, the heat-resistant agent, etc. are effectively dispersed, and the strength and heat resistance of the silicone rubber material are further improved; by using a suitable and effective heat-resistant agent, the thermal conductivity and free radicals are improved, and the long-term high temperature resistance of the silicone rubber is maximized;
[0026] The present invention achieves good processing performance of the mixed rubber through the coordination of the formula and the process, with little loss of performance after heat resistance, and a long service life of the product in long-term reciprocating motion at high temperature. The performance of the silicone rubber material obtained by using domestic methyl vinyl 110 silicone rubber as the raw rubber and optimizing the formula exceeds that of the formula using imported raw rubber as the carrier, and the material can withstand an extreme high temperature of 200°C and reciprocate at a high temperature of 125°C for 2 months without cracks. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is described in detail below through specific embodiments.
[0028] In the following examples, MVQ raw rubber is 110 raw rubber from Bluestar Silicone, and its relative molecular weight is 60-80×10 4 , the vinyl content is 0.03-0.1%; the Qiangwei powder is the vinyl silane modified Qiangwei powder NKL-9 from Shanghai Qixiang; the mercaptosilane coupling agent is the American Momentive mercaptosilane coupling agent NXT.
[0029] Example 1
[0030] A silicone rubber material for a high temperature and fatigue resistant steering protective sleeve, comprising the following raw materials in parts by weight: 50 parts of MVQ raw rubber, 20 parts of modified fumed silica, 1.5 parts of structure control agent D4, 6 parts of Qiangwei powder, 0.7 parts of double 2,5, 0.5 parts of Wacker H0 heat resistant agent, 0.7 parts of red iron oxide, and 0.5 parts of black masterbatch;
[0031] The preparation method of modified fumed silica is as follows: atomizing the mercaptosilane coupling agent through a pressure device and then uniformly spraying it into the fumed silica, reacting at 125°C for 2h, wherein the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:3; the BET value of the fumed silica is 200-230m 2 / g.
[0032] The preparation method of silicone rubber material is:
[0033] S1. Prepare materials by mass, mix MVQ raw rubber, structure control agent D4, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, red iron oxide, and black masterbatch to obtain a premixed rubber. The mixing temperature is 125°C, the speed is 40r / min, and the time is 6h.
[0034] S2. First, add double 2,5 to the premixed rubber for secondary mixing. The temperature of the secondary mixing is 20℃, the speed is 30r / min, and the time is 20min. Then put it in the mold of the vulcanization equipment for primary vulcanization to obtain a primary vulcanized rubber. The primary vulcanization temperature is 170℃, the time is 260s, and the pressure is 150Kgf / cm 2 ;
[0035] S3. Place the primary vulcanized rubber in an oven for secondary vulcanization to obtain the secondary vulcanized rubber; the temperature of the secondary vulcanization is 200°C and the time is 4 hours.
[0036] Example 2
[0037] A silicone rubber material for a high temperature and fatigue resistant steering protective sleeve, comprising the following raw materials in parts by weight: 53 parts of MVQ raw rubber, 22 parts of modified fumed silica, 8 parts of Qiangwei powder, 2.5 parts of structure control agent D4, 1.0 parts of vulcanizing agent di-2,5, 0.7 parts of Wacker H0 heat resistant agent, 1.1 parts of red iron oxide, and 0.5 parts of black masterbatch;
[0038] The preparation method of modified fumed silica is as follows: atomizing the mercaptosilane coupling agent through a pressure device and then uniformly spraying it into the fumed silica, reacting at 130° C. for 2 hours to obtain the modified fumed silica, wherein the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:4; the BET value of the fumed silica is 200-230m 2 / g.
[0039] The preparation method of silicone rubber material is:
[0040] S1. Prepare materials by mass, mix MVQ raw rubber, structure control agent D4, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, red iron oxide, and black masterbatch to obtain a premixed rubber. The mixing temperature is 130°C, the speed is 40r / min, and the time is 6h.
[0041] S2, first add double 2,5 to the premixed rubber for secondary mixing, the secondary mixing temperature is 30℃, the speed is 30r / min, the time is 20min, then put it in the mold of the vulcanization equipment for primary vulcanization to obtain the primary vulcanized rubber, the primary vulcanization temperature is 170℃, the time is 290s, and the pressure is 150Kgf / cm 2 ;
[0042] S3. Place the primary vulcanized rubber in an oven for secondary vulcanization to obtain the secondary vulcanized rubber; the temperature of the secondary vulcanization is 200°C and the time is 4 hours.
[0043] Example 3
[0044] A silicone rubber material for a high temperature and fatigue resistant steering protective sleeve, comprising the following raw materials in parts by weight: 55 parts of VMQ raw rubber, 22 parts of modified fumed silica, 10 parts of Qiangwei powder, 2.5 parts of structure control agent D4, 0.6 parts of vulcanizing agent di-2,5, 0.4 parts of vulcanizing agent 230XL, 1 part of Wacker H0 heat resistant agent, 1.3 parts of red iron oxide, and 0.5 parts of black masterbatch;
[0045] The preparation method of modified fumed silica is as follows: atomizing the mercaptosilane coupling agent through a pressure device and then uniformly spraying it into the fumed silica, reacting at 135° C. for 1.5 hours to obtain the modified fumed silica, wherein the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:5; the BET value of the fumed silica is 200-230m 2 / g.
[0046] The preparation method of silicone rubber material is:
[0047] S1. Prepare materials by mass, mix MVQ raw rubber, structure control agent D4, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, red iron oxide, and black masterbatch to obtain a premixed rubber. The mixing temperature is 130°C, the speed is 40r / min, and the time is 6h.
[0048] S2. First, add double 2,5 and vulcanizer 230XL to the premixed rubber for secondary mixing. The temperature of the secondary mixing is 40℃, the speed is 30r / min, and the time is 20min. Then put it in the mold of the vulcanizing equipment for primary vulcanization to obtain a primary vulcanized rubber. The primary vulcanization temperature is 170℃, the time is 280s, and the pressure is 150Kgf / cm 2;
[0049] S3. Place the primary vulcanized rubber in an oven for secondary vulcanization to obtain the secondary vulcanized rubber; the temperature of the secondary vulcanization is 200°C and the time is 4 hours.
[0050] Example 4
[0051] A silicone rubber material for a high-temperature and fatigue-resistant steering protective sleeve comprises the following raw materials in parts by mass: 58 parts of MVQ raw rubber, 24 parts of modified fumed silica, 10 parts of Qiangwei powder, 2.5 parts of structure control agent D4, 0.6 parts of vulcanizing agent di-2,5, 0.7 parts of vulcanizing agent 230XL, 1.2 parts of Wacker H0 heat resistant agent, 1.3 parts of red iron oxide, and 0.5 parts of black masterbatch.
[0052] The preparation method of modified fumed silica is as follows: atomizing the mercaptosilane coupling agent through a pressure device and then uniformly spraying it into the fumed silica, reacting at 130°C for 2h, wherein the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:6; the BET value of the fumed silica is 200-230m 2 / g.
[0053] The preparation method of silicone rubber material is:
[0054] S1. Prepare materials by mass, mix MVQ raw rubber, structure control agent D4, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, red iron oxide, and black masterbatch to obtain a premixed rubber. The mixing temperature is 130°C, the speed is 40r / min, and the time is 6h.
[0055] S2. First, add double 2,5 and vulcanizing agent 230XL to the premixed rubber for secondary mixing. The temperature of the secondary mixing is 30℃, the speed is 30r / min, and the time is 20min. Then put it in the mold of the vulcanizing equipment for primary vulcanization to obtain a primary vulcanized rubber. The primary vulcanization temperature is 165-180℃, the time is 300s, and the pressure is 160Kgf / cm 2 ;
[0056] S3. Place the primary vulcanized rubber in an oven for secondary vulcanization to obtain the secondary vulcanized rubber; the temperature of the secondary vulcanization is 200°C and the time is 4 hours.
[0057] Example 5
[0058] A high-temperature and fatigue-resistant silicone rubber material for a steering protective sleeve comprises the following raw materials in parts by weight: 58 parts of MVQ raw rubber, 26 parts of modified fumed silica, 6 parts of Qiangwei powder, 4.0 parts of structure control agent D4, 1.0 parts of vulcanizing agent 230XL, 1.2 parts of Wacker H0 heat-resistant agent, 1 part of nano cerium oxide, 1 part of red iron oxide, and 0.5 parts of black masterbatch.
[0059] The preparation method of modified fumed silica is as follows: atomizing the mercaptosilane coupling agent through a pressure device and then uniformly spraying it into the fumed silica, reacting at 130°C for 2h, wherein the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:7; the BET value of the fumed silica is 200-230m 2 / g.
[0060] The preparation method of silicone rubber material is:
[0061] S1. Prepare materials by mass, mix MVQ raw rubber, structure control agent D4, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, nano cerium oxide, red iron oxide, and black masterbatch to obtain a premixed rubber. The mixing temperature is 130° C., the speed is 40 r / min, and the time is 6 h.
[0062] S2. First, add the vulcanizing agent 230XL to the premixed rubber for secondary mixing. The temperature of the secondary mixing is 40°C, the speed is 30r / min, and the time is 20min. Then, place it in the mold of the vulcanizing equipment for primary vulcanization to obtain a primary vulcanized rubber. The primary vulcanization temperature is 170°C, the time is 300s, and the pressure is 150Kgf / cm 2 ;
[0063] S3. Place the primary vulcanized rubber in an oven for secondary vulcanization to obtain the secondary vulcanized rubber; the temperature of the secondary vulcanization is 200°C and the time is 4 hours.
[0064] Example 6
[0065] A high-temperature and fatigue-resistant silicone rubber material for a steering protective sleeve comprises the following raw materials in parts by weight: 60 parts of MVQ raw rubber, 30 parts of modified fumed silica, 26 parts of Qiangwei powder, 8 parts of structure control agent D4, 1.3 parts of vulcanizing agent 230XL, 1.5 parts of Wacker H0 heat-resistant agent, 1 part of nano cerium oxide, 1.5 parts of red iron oxide, and 0.5 parts of black masterbatch.
[0066] The preparation method of modified fumed silica is as follows: atomizing the mercaptosilane coupling agent through a pressure device and then uniformly spraying it into the fumed silica, reacting at 130°C for 2h, wherein the mass ratio of the fumed silica to the mercaptosilane coupling agent is 100:8; the BET value of the fumed silica is 200-230m 2 / g.
[0067] The preparation method of silicone rubber material is:
[0068] S1. Prepare materials by mass, mix MVQ raw rubber, structure control agent D4, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, nano cerium oxide, red iron oxide, and black masterbatch to obtain a premixed rubber. The mixing temperature is 125°C, the speed is 40r / min, and the time is 6h;
[0069] S2. First, add the vulcanizing agent 230XL to the premixed rubber for secondary mixing. The temperature of the secondary mixing is 0°C, the speed is 30r / min, and the time is 20min. Then, place it in the mold of the vulcanizing equipment for primary vulcanization to obtain a primary vulcanized rubber. The primary vulcanization temperature is 170°C, the time is 300s, and the pressure is 155Kgf / cm 2 ;
[0070] S3. Place the primary vulcanized rubber in an oven for secondary vulcanization to obtain the secondary vulcanized rubber; the temperature of the secondary vulcanization is 200°C and the time is 4 hours.
[0071] Comparative Example 1
[0072] The only difference between Comparative Example 1 and Example 1 is that the raw material of the silicone rubber material does not contain Wacker H0 heat resistant agent.
[0073] Comparative Example 2
[0074] The only difference between Comparative Example 2 and Example 1 is that the raw material of the silicone rubber material does not contain red iron oxide.
[0075] Comparative Example 3
[0076] The difference between Comparative Example 3 and Example 1 is that the fumed silica used is different; the BET value of the fumed silica used in Comparative Example 3 is 155-175m 2 / g.
[0077] Comparative Example 4
[0078] The difference between Comparative Example 4 and Example 1 is only that the silane coupling agent used to prepare the modified fumed silica is different; Comparative Example 4 uses bis(γ-triethoxysilylpropyl)tetrasulfide, and the preparation method of the modified fumed silica in Comparative Example 4 is: bis(γ-triethoxysilylpropyl)tetrasulfide is atomized by a pressure device and then evenly sprayed on the fumed silica, and reacted at 125° C. for 2 hours to obtain, wherein the mass ratio of fumed silica to bis(γ-triethoxysilylpropyl)tetrasulfide is 100:3; the BET value of the fumed silica is 200-230m 2 / g.
[0079] Comparative Example 5
[0080] The difference between Comparative Example 5 and Example 1 is that in S1, the process of the first mixing is different, specifically, the temperature of the first mixing is 145° C., the rotation speed is 40 r / min, and the time is 2.5 h.
[0081] Test example
[0082] The performance of the silicone rubber materials of Examples 1-6 was tested, and the test results are shown in Table 1:
[0083] Table 1
[0084]
[0085]
[0086] The performance of the silicone rubber materials of Comparative Examples 1-5 was tested, and the test results are shown in Table 2:
[0087] Table 2
[0088]
[0089]
[0090] In the present invention, MVQ is selected as the raw rubber matrix. In a suitable vulcanization system, with the aid of a suitable protection system and preparation process, the heat-resistant temperature of MVQ can be increased to 200°C. The obtained high-temperature dynamic protective cover material has high tensile strength and elongation, excellent long-term high-temperature resistance and dynamic fatigue performance, excellent processing technology, and long practical validity period. It can be used to manufacture protective cover rubber products with high-temperature dynamic requirements such as automotive hoses, water pump supports, high-heat-resistant protective covers, high-heat-resistant sealing strips and engine connecting pipes.
[0091] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high temperature and fatigue resistant silicone rubber material for a steering protective sleeve, characterized in that: The invention comprises the following raw materials in parts by weight: 50-60 parts of MVQ raw rubber, 20-40 parts of modified fumed silica, 5-30 parts of Qiangwei powder, 1-8 parts of structure control agent, 0.5-1.5 parts of vulcanizing agent, 0.5-2 parts of Wacker H0 heat resistant agent, 0.5-2.5 parts of metal oxide heat resistant agent, and 0.3-1 parts of black masterbatch; The modified fumed silica is obtained by surface-modifying fumed silica with a mercaptosilane coupling agent, wherein the BET value of the fumed silica is 200-400 m 2 / g.
2. The high temperature and fatigue resistant silicone rubber material for steering protection sleeve according to claim 1, characterized in that: The MVQ raw rubber is 110 methyl vinyl silicone rubber; preferably, the vinyl content of the 110 methyl vinyl silicone rubber is 0.03-0.1%.
3. The high temperature and fatigue resistant silicone rubber material for steering protection sleeve according to claim 1, characterized in that: The Qiangwei powder is vinyl silane modified Qiangwei powder; the structure control agent is octamethylcyclotetrasiloxane; the vulcanizing agent is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 4,4-di(tert-butylperoxy)butyl valerate or a combination thereof; the metal oxide heat resistant agent is nano-grade cerium oxide, red iron oxide or a combination thereof.
4. A method for preparing a high temperature and fatigue resistant silicone rubber material for a steering protective sleeve according to any one of claims 1 to 3, characterized in that: The steps include: S1. Prepare materials by mass, and mix MVQ raw rubber, structure control agent, modified fumed silica, Qiangwei powder, Wacker H0 heat resistant agent, metal oxide heat resistant agent, and black masterbatch to obtain a premixed rubber; S2, first add the vulcanizing agent to the premixed rubber for secondary mixing, and then perform a vulcanization in the mold to obtain a primary vulcanized rubber; S3, subjecting the primary vulcanized rubber to secondary vulcanization to obtain.
5. The method for preparing the high temperature and fatigue resistant silicone rubber material for steering protective sleeve according to claim 4, characterized in that: In S1, the temperature of the first mixing is 110-130°C, the rotation speed is 20-50r / min, and the time is 3-8h; in S2, the temperature of the second mixing is 0-40°C, the rotation speed is 20-50r / min, and the time is 5-30min.
6. The method for preparing the high temperature and fatigue resistant silicone rubber material for steering protective sleeve according to claim 4, characterized in that: In S3, the primary vulcanization temperature is 160-180℃, the time is 160-320s, and the pressure is 140-180Kgf / cm 2 .
7. The method for preparing the high temperature and fatigue resistant silicone rubber material for steering protective sleeve according to claim 4, characterized in that: In S3, the temperature of the secondary vulcanization is 180-200°C and the time is 2-4h.
8. A high temperature and fatigue resistant silicone rubber material for a steering protective sleeve, characterized in that: Prepared by the preparation method according to any one of claims 4 to 7.