Efficient polishing abrasive particle flow slurry and preparation method thereof
Through the combination of silicon carbide abrasive particles and dispersant with a specific particle size distribution, the problem of difficulty in taking into account the viscosity and solid phase content in abrasive flow polishing is solved, efficient polishing and stable dispersion are achieved, and surface roughness and inner flow channels are reduced. Risk of deformation.
Patent Information
- Application Number
- CN202411079518.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing abrasive flow polishing technology, it is difficult to achieve the low viscosity and high solid phase content of the silicon carbide suspension at the same time, resulting in low polishing efficiency, and abrasive particles are prone to accumulate and blockage in complex inner flow channels, resulting in increased surface residual stress and micro-small stress. crack.
Silicon carbide abrasive particles (300-500nm, 0.8-1.2μm and 4-5μm) with specific particle size distribution combined with polyethyleneimine dispersant and ethanol, and the pH value and particle ratio are adjusted through ultrasonic and ball mill dispersion treatment to form The stable abrasive slurry ensures that the abrasive particles are dispersed in water for a long time, reduces viscosity, and improves polishing efficiency.
The stable dispersion and efficient polishing of silicon carbide particles are achieved, the surface roughness of the material is reduced, the inner channel deformation and polishing defects are avoided, and the processing efficiency and product quality are improved.
Smart Images

Figure CN118995052A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of precision machining, and specifically relates to an abrasive flow slurry for efficient polishing and a preparation method thereof, in particular to an abrasive flow slurry for efficient polishing of complex internal flow channels and a preparation method thereof. Background Art
[0002] In recent years, the rapid development of high-precision manufacturing technology represented by aerospace has driven parts to develop in the direction of high precision and complex structure. However, traditional processing methods have limitations in polishing, chamfering and deburring the surface and interior of parts, and cannot process and manufacture such parts. Therefore, a new special processing technology, abrasive flow polishing, is proposed to perform precision processing on channel parts.
[0003] Abrasive flow has broad application prospects and various advantages in the field of micro-porous flow channel processing, but there are also various problems that need to be solved urgently: when the abrasive flow slurry used has poor stability, the abrasive particles will remain in the bends, dead corners or intersection nodes of the complex flow channels after grinding, and the metal powder and even abrasive particles cut off will accumulate and clog these areas, making subsequent processing impossible; there are obvious macroscopic forces in the abrasive flow polishing process. If the slurry viscosity is high, the residual stress on the workpiece surface after polishing will increase significantly, which can easily cause deformation of the inner flow channel and even produce microcracks when processing thin-walled inner flow channels.
[0004] In summary, low viscosity, high solid content and relatively good stability are important conditions to ensure the efficiency of abrasive flow polishing. However, due to the non-wetting characteristics of the interface between abrasive powder and water, it is difficult for the two to form a relatively stable interface, making it difficult for the abrasive to be stably and evenly dispersed in water. It is very easy to settle and accumulate at the bottom of the suspension in a muddy state with high viscosity. Therefore, it is difficult to achieve low viscosity and high solid content of silicon carbide suspension at the same time. However, current research on abrasive flow polishing is mostly focused on the optimization of process and equipment, and there is less work on the optimization of slurry properties. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an abrasive flow slurry for efficient polishing and a preparation method thereof, so as to solve the problem of low polishing efficiency caused by the difficulty in simultaneously achieving low viscosity and high solid content of silicon carbide suspension. This method can make silicon carbide particles disperse stably in water for a long time, increase the abrasive content while reducing viscosity, and improve polishing efficiency; further, the material obtained by polishing using this slurry has low roughness.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing an abrasive flow slurry for efficient polishing comprises the following steps:
[0008] Step 1, mixing silicon carbide abrasive particles of three grades with particle sizes of 300-500 nm, 0.8-1.2 μm and 4-5 μm in water, wherein the mass ratio of the silicon carbide abrasive particles of three grades with particle sizes of 300-500 nm, 0.8-1.2 μm and 4-5 μm is (10-30): (20-40): (40-70); adding a polyethyleneimine dispersant, adjusting the pH value, and adding ethanol to obtain a mixed slurry;
[0009] Step 2: subjecting the mixed slurry to ultrasonic dispersion and ball milling dispersion treatment in sequence to obtain a high-efficiency polishing abrasive flow slurry.
[0010] A further improvement of the present invention is:
[0011] Preferably, in step 1, the mass ratio of the total mass of silicon carbide abrasive grains, water and ethanol is (75-125): (75-125): (3-5).
[0012] Preferably, in step 1, the pH value of the slurry is adjusted to 4-10.
[0013] Preferably, in step 1, the pH value is adjusted by using hydrochloric acid and sodium silicate aqueous solution.
[0014] Preferably, in step 1, the mass fraction of the polyethyleneimine dispersant in the slurry is 0.25-0.35%.
[0015] Preferably, in step 2, the ultrasonic dispersion power is 150-220 W, and the ultrasonic dispersion time is ≥10 min.
[0016] Preferably, in step 2, the ball milling dispersion speed is 200 to 300 rpm, and the ball milling dispersion time is 5 to 10 h.
[0017] An abrasive flow slurry for high-efficiency polishing prepared by any one of the preparation methods described above, wherein the slurry contains silicon carbide abrasive grains of three grades with particle sizes of 300-500nm, 0.8-1.2μm and 4-5μm.
[0018] Preferably, the mass fraction of silicon carbide abrasive particles in the slurry is 50%.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention discloses a method for preparing an abrasive flow slurry for efficient polishing. The slurry is based on the high hardness characteristics of SiC materials and is intended to achieve efficient grinding and polishing of the inner wall of a workpiece. In the preparation process, silicon carbide ceramic abrasive particles with a specific particle size distribution are selected, and the particle size ranges are 300-500nm, 0.8-1.2μm and 4-5μm, respectively, and the mass ratio of the three particle size abrasive particles is limited. Through the matching of particles of three particle sizes and weight limitation, the stability and fluidity of the abrasive particles in the slurry system are ensured, and the rapid sinking caused by excessive particle mass is avoided, and the agglomeration and sedimentation caused by excessive specific surface area are also prevented. At the same time, the polishing efficiency of large particle size and the polishing accuracy of small particle size are taken into account. The lubrication effect of small particles on the flow process of large particles is utilized to reduce the viscosity of the system, improve the fluidity of the slurry, and enable the slurry to evenly polish the complex internal flow channel. At the same time, the electrostatic repulsion on the surface of the particles when dispersed in water and the steric stabilization effect of the dispersant macromolecules are utilized to make the silicon carbide particles stably dispersed in water over a long period of time; the lubricating effect of small particles on large particles is utilized to obtain a lower viscosity at a higher solid content, and a low-viscosity and high-solid content slurry is obtained, which makes it easy to grind and polish the inner wall of the workpiece with complex flow channels at a lower pressure.
[0021] The invention also discloses a ceramic slurry for efficient polishing, which has the characteristics of high solid content, low viscosity and good wettability. The material obtained by abrasive flow polishing with the slurry has low surface roughness, good structural uniformity and no polishing defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The flowchart of obtaining the ceramic slurry for efficient polishing of the present invention;
[0023] Figure 2 The inner hole morphology and roughness results of the workpiece before and after polishing. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0025] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0026] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0027] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0028] The first aspect of the present invention discloses an abrasive flow slurry for efficient polishing, wherein the silicon carbide ceramic slurry comprises silicon carbide abrasive grains, a polyethyleneimine dispersant, ethanol, hydrogen chloride, sodium silicate and water; wherein the silicon carbide abrasive grains are composed of silicon carbide abrasive grains of three grades with particle sizes of 300-500nm, 0.8-1.2μm and 4-5μm, wherein the silicon carbide ceramic abrasive grains in the slurry will neither rapidly and spontaneously sink in the system due to excessive particle mass, nor rapidly agglomerate and settle in the system due to excessive specific surface area, nor be unable to be stably suspended due to excessive mass, and at the same time, the electrostatic repulsion on the surface of the particles when dispersed in water and the steric stabilizing effect of the polyethyleneimine dispersant macromolecules are utilized to stably disperse the silicon carbide particles in water over a long period of time, the three particle sizes of abrasive grains are evenly mixed and nested with each other, thereby ensuring the density of the abrasive slurry, and obtaining a slurry with low viscosity and high solid content, which makes it easy to grind and polish the inner wall of a workpiece with a complex flow channel at a relatively low pressure.
[0029] Some embodiments of the present invention In some embodiments of the present invention, the mass ratio of abrasive, water and ethanol is (75-125): (75-125): (3-5); this ratio ensures that the slurry has good fluidity and stability, while avoiding too fast sedimentation or agglomeration of the abrasive.
[0030] In some embodiments of the present invention, in order to further improve the stability of the slurry, a polyethyleneimine dispersant is added thereto. Based on the total mass of the ceramic slurry (100%), the mass fraction of the polyethyleneimine dispersant is controlled between 0.25% and 0.35%. The dispersant effectively prevents the mutual aggregation of silicon carbide abrasive particles through its electrostatic repulsion and steric hindrance effect.
[0031] The pH value of the slurry is one of the key factors affecting the dispersion effect. In some embodiments of the present invention, deionized water (pH value is about 7) is used as a solvent in the initial state. In order to adjust the pH value of the slurry to the optimal range (4 to 10), an appropriate amount of hydrogen chloride (for lowering the pH value) or sodium silicate (for increasing the pH value) is added according to actual needs. The specific amount added needs to be determined through experiments to ensure that the slurry achieves the desired stability and dispersion effect.
[0032] In some embodiments of the present invention, among the silicon carbide abrasive particles, the mass ratio of the three types of silicon carbide abrasive particles of 300-500nm, 0.8-1.2μm and 4-5μm is (10-30): (20-40): (40-70). Specific surface area is the ratio of the surface area of a particle to its volume. Generally speaking, the smaller the particle size, the larger the specific surface area. This is because the smaller the diameter of the particle, the more particles there are per unit volume, and the larger the total surface area, resulting in an increase in specific surface area. Particles with large specific surface areas tend to have higher surface energy and are easily attracted to each other and agglomerated. In the present invention, by adjusting the weight ratio of the three levels of abrasive particles, the surface energy of the abrasive particles can be reduced, the attraction between them can be reduced, and agglomeration and sedimentation can be avoided.
[0033] Preferably, the mass ratio of 300-500 nm, 0.8-1.2 μm and 4-5 μm silicon carbide abrasive particles is 10:20:70;
[0034] As one of the preferred embodiments, when the pH value of the slurry is 8 and the mass fraction of the polyethyleneimine dispersant is 0.3%, the viscosity performance and stability of the slurry are the best.
[0035] The invention also discloses a method for preparing a ceramic slurry for efficient polishing. The slurry obtained by the method has the characteristics of high solid content, low viscosity and good wettability. The material obtained by abrasive flow polishing with the slurry has low surface roughness, good structural uniformity and no polishing defects.
[0036] The second aspect of the present invention discloses a method for preparing an abrasive flow slurry for high-efficiency polishing, the preparation method comprising the following steps:
[0037] Step 1, pouring silicon carbide abrasive grains with particle sizes of 300-500 nm, 0.8-1.2 μm and 4-5 μm into a beaker filled with deionized water, adding a certain mass fraction of polyethyleneimine aqueous solution, adjusting the pH of the suspension with hydrochloric acid and sodium silicate aqueous solution, and then adding ethanol to obtain a mixed slurry;
[0038] The mass ratio of silicon carbide, water and ethanol is (75-125): (75-125): (3-5); based on the mass of the ceramic slurry being 100%, the mass fraction of the polyethyleneimine aqueous solution in the entire slurry is 0.25-0.35%;
[0039] Preferably, the mass ratio of anhydrous ethanol to water is 1:20. Anhydrous ethanol and deionized water are mixed in a certain proportion to improve the antibacterial properties of the slurry during the infiltration process. The configured slurry needs to be stored for a long time. However, ethanol is volatile. Under the premise of ensuring wettability, the ethanol content in the whole system should be reduced as much as possible to maintain good stability of the slurry. Preferably, the volume ratio of anhydrous ethanol to deionized water is 1:20.
[0040] Step 2, subjecting the mixed slurry to ultrasonic dispersion and ball milling dispersion treatment in sequence to obtain silicon carbide ceramic slurry;
[0041] The ultrasonic dispersion power is 150-220W, preferably, the ultrasonic dispersion power is 195W; the ultrasonic dispersion time is >10min;
[0042] Preferably, the stirring speed of the ball milling dispersion is 200 to 300 rpm; and the time of the ball milling dispersion is 5 to 10 hours.
[0043] Preferably, the mass fraction of silicon carbide abrasive particles in the finally obtained silicon carbide ceramic slurry is 50%.
[0044] See also Figure 1 One embodiment of the present invention discloses a test method for obtaining the above-mentioned abrasive flow slurry ratio, comprising the following steps:
[0045] S1. A small amount of ceramic powder is mixed with deionized water, and different mass fractions of polyethyleneimine (PEI) aqueous solutions are added respectively, and the pH and mass ratios of three different particle sizes are adjusted to obtain several sets of orthogonal condition parameter dilute solutions.
[0046] The solid mass fraction of the suspension in S1 is 0.05% to 0.5%. A certain mass fraction of dilute suspension is set to maximize the difference in electrostatic repulsion between particles in suspensions with different parameter conditions, making it easier for the Zeta potential meter to measure the difference. Thus, the best pH value and PEI concentration parameters are selected. Preferably, the solid mass fraction of the suspension is 0.1%.
[0047] The silicon carbide ceramic particles in S1 are of three grades: 300-500nm, 0.8-1.2μm and 4-5μm. For these three grades of particles, different mass ratios are used as variables; the pH parameter range is selected as 4-10, and the PEI mass fraction range is selected as 0-0.4%. The appropriate particle size allows the electrostatic force of the particles in the liquid to offset gravity, without aggregation and sedimentation. The appropriate pH value will increase the electrostatic repulsion between particles and strengthen the electrostatic steric effect. The appropriate dispersant concentration guides the increase in the distance between particles, constrains the particle activity space, and strengthens the steric hindrance effect. The electrostatic stabilization mechanism and the steric stabilization mechanism generated by the dispersant work together to reduce the viscosity of the slurry. The two conditions of the parameter pH value and PEI concentration are orthogonally combined into 7 groups of test suspensions, and the Zeta potential value is measured by a Malvern Zeta potential meter.
[0048] S2. Measure the zeta potential of the orthogonal solution group, select the group with the largest absolute value of zeta potential and record it; according to the orthogonal test results, when the mass ratio of 300-500nm, 0.8-1.2μm and 4-5μm silicon carbide abrasives is 10:20:70, the slurry pH value is 8±0.2, and the mass fraction of dispersant PEI is (0.3±0.05)%, the absolute value of zeta potential is the largest, reaching 57.3mV.
[0049] S3. Prepare an abrasive flow slurry with a mass fraction of 50%, and use the optimal values obtained in S2 as parameters for adjusting pH and PEI concentration.
[0050] The volume ratio of anhydrous ethanol and dispersant deionized water added to S3 is 1:10-40.
[0051] S4. The mixed slurry is first dispersed by ultrasonic, then poured into a planetary ball mill and stirred for 4 hours to obtain the desired slurry.
[0052] The present invention is aimed at the polishing inside complex internal flow channels, and has strict requirements on the dispersion of the polishing materials, and challenges of complex interactions between particles and liquid media. These effects include but are not limited to van der Waals forces, Coulomb forces, solvent effects, capillary forces, hydrophobic forces and hydrodynamic forces, which together shape the behavior of particles in liquids. What is particularly critical is that the surface charge state of the particles has a decisive influence on the dispersion effect. Small-sized particles are easy to aggregate and settle due to their large specific surface area, while large-sized particles tend to settle by gravity due to the weakening of microscopic forces. The present invention is the first to use abrasives of three particle sizes in combination, and to limit the mass ratio of the three particle sizes of abrasives, so that the final abrasive particles have a suitable specific surface area as a whole, and can balance gravity during the polishing process, and have stable dispersion.
[0053] Particles with a wider size distribution tend to pack better than similar suspended particles with a narrower size distribution. In the case of a wider particle size distribution, there is usually more free space for individual particles to move around. This makes the sample more fluid. This also means that the viscosity of the material is lower. Therefore, the viscosity and stability of suspension-type materials can be improved by reducing the particle size distribution. When the mass fraction remains constant, samples containing both large and small particles tend to have lower viscosity values than samples containing only large particles or only small particles. This is mainly related to two factors. One is related to the degree of interaction between the particles. When the particle size decreases, the degree of interaction between the particles increases, so the viscosity value of the material also increases. Another factor is that the viscosity value of the material decreases as the particle size distribution increases. In this case, the particle size distribution has a more significant effect on the viscosity reduction.
[0054] The present invention takes into account steric hindrance, static electricity and the quality of particles of three sizes, and jointly adjusts the comprehensive influence of suspension viscosity and stability. The slurry particles of three particle sizes finally obtained are evenly dispersed in every corner of the system. There is no precipitation caused by the internal microscopic force being insufficient to offset its gravity due to the large particle diameter, nor is there agglomeration and sedimentation caused by the particle diameter being too small. Under the joint action of the appropriate mass ratio of particles of different particle sizes, dispersant concentration and pH, the effects of the steric hindrance stabilization mechanism and the electrostatic stabilization mechanism are maximized. The gravity, electrostatic force and spatial resistance exerted on the particles inside the dispersed system maintain a relative balance, so that the suspension can exist stably for a long time.
[0055] Example 1
[0056] A method for preparing an abrasive flow slurry comprises the following steps:
[0057] S1. Pour silicon carbide abrasive grains with a grain size ratio of 300-500nm: 0.8-1.2μm: 4-5μm = 10:20:70 into a beaker filled with deionized water, the mass ratio of silicon carbide abrasive grains to deionized water is 1:1, add a polyethyleneimine aqueous solution with a mass fraction of 10%, adjust the pH of the suspension to 8 using hydrochloric acid with a pH value of 2 and a sodium silicate aqueous solution with a hydrochloric acid value of 12, and then add ethanol to obtain a mixed slurry; wherein the mass fraction of the polyethyleneimine aqueous solution in the mixed slurry is 0.3%, and the amount of ethanol added is 5% of the mass of the mixed slurry, so that the mass ratio of silicon carbide abrasive grains: deionized water and ethanol is 75:75:5.
[0058] S2. The mixed slurry is subjected to ultrasonic dispersion and ball milling dispersion treatment in sequence to obtain silicon carbide ceramic slurry; the ultrasonic dispersion power is 195W, the working time is set to 2 seconds, the interval is 1 second, the total dispersion time is 10 minutes, the orbital speed of the planetary ball mill during stirring is 100rpm, the rotation speed is 200rpm, the stirring time is 5h, and the forward and reverse rotations are turned on.
[0059] The slurry density prepared in this embodiment is 2.6 g / cm 3 , viscosity is 10mPa·s.
[0060] In this embodiment, a suitable mass ratio is set for silicon carbide abrasive particles of three levels of particle size, so that the electrostatic force of the particles in the liquid can offset the gravity, and no aggregation and sedimentation occur. pH = 8 can increase the electrostatic repulsion between particles and strengthen the electrostatic steric effect. The mass fraction of the dispersant is 0.3%, which can guide the increase of the distance between particles, constrain the activity space of the particles, and strengthen the steric effect. The electrostatic stabilization mechanism and the steric stabilization mechanism generated by the dispersant work together to reduce the viscosity of the slurry. The Zeta potential value was measured by a Malvern Zeta potential meter, and the absolute value of the zeta potential prepared by this embodiment was 57.3mV.
[0061] See also Figure 2 For the application of this embodiment, the surface roughness change and surface morphology of the inner hole of the sample before and after abrasive flow polishing are shown in the figure. It can be seen from the figure that the surface is obviously smoother.
[0062] Comparative Example 1
[0063] The difference from Example 1 is:
[0064] The abrasive particle size ratio of the silicon carbide ceramic slurry is: 300-500nm: 0.8-1.2μm: 4-5μm: 50-60μm = 20:20: (30-50) 40:20.
[0065] The rest is the same as Example 1 and will not be described again here.
[0066] Comparative Example 2
[0067] The difference from Example 1 is:
[0068] The abrasive particle size ratio of the silicon carbide ceramic slurry is: 50-100nm: 300-500nm: 0.8-1.2μm: 4-5μm: 50-60μm=15:15:20:40:10.
[0069] The rest is the same as Example 1 and will not be described again here.
[0070] Comparative Example 3
[0071] The difference from Example 1 is:
[0072] The abrasive particle size ratio of the silicon carbide ceramic slurry is: 50-100nm: 300-500nm: 0.8-1.2μm: 4-5μm=15:15:20:50.
[0073] The rest is the same as Example 1 and will not be described again here.
[0074] 1. Viscosity test: At 25°C, take 20 mL of the prepared slurry at the first time. Pour it into the standard measuring cylinder of NDJ-1S rotary viscometer. Use rotor No. 0 to measure the viscosity of the slurry under four gradient conditions of rotor speed 60RPM, 30RPM, 12RPM, and 6RPM. Take the value of 30% to 50% of the range of the corresponding rotor speed as the viscosity measurement value of the slurry in this embodiment.
[0075] 2. Stability test: Pour the measured viscosity slurry into 15mL sample bottles, seal them, mark them in order, and place them under the same external conditions to stand, and record the sedimentation and stratification of the slurry every 1 hour. When a clear liquid-solid interface is observed in the sample bottle, record it as the sedimentation time of the slurry of this embodiment. The performance comparison of each embodiment after viscosity test and stability test is shown in Table 1:
[0076] Table 1 Parameters and performances of various embodiments
[0077] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Viscosity value / mPa·s 4.62 3.21 3.64 7.51 Sedimentation time / min 67 14 36 24
[0078] As can be seen from Table 1 above, the present invention has lower viscosity and higher stability than the existing slurry used for abrasive flow polishing. Compared with Comparative Examples 1 and 2, the addition of 50-60μm abrasive particles reduces the overall viscosity of the slurry, but because it is basically not constrained by the electrostatic force in the suspension, it settles quickly after addition, resulting in poor stability of the two groups of slurries. And based on the application background of the present invention in grinding and polishing of laser drilling, the processed aperture is small, so the abrasive particle size should not be too large to avoid polishing defects. Comparing Example 1 and Comparative Example 3, after the 50-100nm particle size slurry with too low particle size is added to the slurry system, due to its large specific surface area, the agglomeration phenomenon between the particles is obvious. It is difficult to separate it in the abrasive state and form a stable interface with water, so it is difficult to disperse in water. Even if a small part is dissolved in water, it will soon reunite with adjacent particles to form a paste-like substance. This has a greater impact on the overall particle dispersion of the abrasive flow slurry, so the present invention ultimately selects only three types of abrasives: 300-500nm, 0.8-1.2μm and 4-5μm.
[0079] Example 2
[0080] In this embodiment, the mass ratio of the three levels of silicon carbide abrasive grains of 300-500 nm, 0.8-1.2 μm and 4-5 μm is 20:40:50, and the rest is the same as that of Embodiment 1 and will not be repeated here.
[0081] Example 3
[0082] In this embodiment, the mass ratio of the three grades of silicon carbide abrasive grains of 300-500 nm, 0.8-1.2 μm and 4-5 μm is 30:40:70, and the rest is the same as that in Embodiment 1 and will not be described again.
[0083] Example 4
[0084] In this embodiment, the mass ratio of the three levels of silicon carbide abrasive grains of 300-500 nm, 0.8-1.2 μm and 4-5 μm is 15:30:60, and the rest is the same as in Embodiment 1 and will not be repeated here.
[0085] Example 5
[0086] In this embodiment, the mass ratio of the three grades of silicon carbide abrasive grains of 300-500 nm, 0.8-1.2 μm and 4-5 μm is 30:40:70, and the rest is the same as that in Embodiment 1 and will not be described again.
[0087] Example 6
[0088] In this embodiment, the mass ratio of the total mass of silicon carbide abrasive grains, water and ethanol is 125:125:5, and the rest is the same as in Embodiment 1 and will not be repeated here.
[0089] Example 7
[0090] In this embodiment, the mass ratio of the total mass of silicon carbide abrasive grains, water and ethanol is 100:110:4, and the rest is the same as in Embodiment 1 and will not be repeated here.
[0091] Example 8
[0092] In this embodiment, the mass ratio of the total mass of silicon carbide abrasive grains, water and ethanol is 80:120:4, and the rest is the same as in Embodiment 1 and will not be repeated here.
[0093] Example 9
[0094] In this embodiment, the pH value of the slurry is 4, and the rest is the same as in Embodiment 1, which will not be described again.
[0095] Example 10
[0096] In this embodiment, the pH value of the slurry is 5, and the rest is the same as in Embodiment 1, which will not be described again.
[0097] Embodiment 11
[0098] In this embodiment, the pH value of the slurry is 10, and the rest is the same as in Embodiment 1, which will not be described again.
[0099] Example 12
[0100] In this embodiment, the mass fraction of the polyethyleneimine dispersant in the slurry is 0.25%, and the rest is the same as in Embodiment 1, which will not be described again.
[0101] Embodiment 13
[0102] In this embodiment, the mass fraction of the polyethyleneimine dispersant in the slurry is 0.35%, and the rest is the same as in Embodiment 1, which will not be described again.
[0103] Embodiment 14
[0104] In this embodiment, the ultrasonic dispersion power is 150W, the ultrasonic dispersion time is 15 minutes, and the rest is the same as in Embodiment 1, which will not be described again.
[0105] Embodiment 15
[0106] In this embodiment, the ultrasonic dispersion power is 220W, the ultrasonic dispersion time is 10 minutes, and the rest is the same as in Embodiment 1, which will not be described again.
[0107] Example 16
[0108] In this embodiment, the ultrasonic dispersion power is 180W, the ultrasonic dispersion time is 15 minutes, and the rest is the same as in Embodiment 1, which will not be described again.
[0109] Embodiment 17
[0110] In this embodiment, the ball milling dispersion rotation speed is 200 rpm, the ball milling dispersion time is 10 h, and the rest is the same as in Example 1, which will not be repeated here.
[0111] Embodiment 18
[0112] In this embodiment, the ball milling dispersion rotation speed is 300 rpm, the ball milling dispersion time is 5 h, and the rest is the same as in Example 1, which will not be repeated here.
[0113] Embodiment 19
[0114] In this embodiment, the ball milling dispersion rotation speed is 250 rpm, the ball milling dispersion time is 8 h, and the rest is the same as in Example 1, which will not be repeated here.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an abrasive flow slurry for high-efficiency polishing, characterized in that: The following steps are involved: Step 1, mixing silicon carbide abrasive particles of three grades with particle sizes of 300-500 nm, 0.8-1.2 μm and 4-5 μm in water, wherein the mass ratio of the silicon carbide abrasive particles of three grades with particle sizes of 300-500 nm, 0.8-1.2 μm and 4-5 μm is (10-30): (20-40): (40-70); adding a polyethyleneimine dispersant, adjusting the pH value, and adding ethanol to obtain a mixed slurry; Step 2: subjecting the mixed slurry to ultrasonic dispersion and ball milling dispersion treatment in sequence to obtain a high-efficiency polishing abrasive flow slurry.
2. The method for preparing a high-efficiency polishing abrasive flow slurry according to claim 1, characterized in that: In step 1, the mass ratio of the total mass of silicon carbide abrasive grains, water and ethanol is (75-125): (75-125): (3-5).
3. The method for preparing a high-efficiency polishing abrasive flow slurry according to claim 1, characterized in that: In step 1, the pH value of the slurry is adjusted to 4-10.
4. The method for preparing a high-efficiency polishing abrasive flow slurry according to claim 1, characterized in that: In step 1, the pH value is adjusted by using hydrochloric acid and sodium silicate aqueous solution.
5. The method for preparing a high-efficiency polishing abrasive flow slurry according to claim 1, characterized in that: In step 1, the mass fraction of the polyethyleneimine dispersant in the slurry is 0.25-0.35%.
6. The method for preparing a high-efficiency polishing abrasive flow slurry according to claim 1, characterized in that: In step 2, the ultrasonic dispersion power is 150-220 W, and the ultrasonic dispersion time is ≥10 min.
7. The method for preparing a high-efficiency polishing abrasive flow slurry according to claim 1, characterized in that: In step 2, the ball milling dispersion speed is 200-300 rpm, and the ball milling dispersion time is 5-10 h.
8. An abrasive flow slurry for high-efficiency polishing prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The slurry contains silicon carbide abrasive grains of three grades, namely, 300-500 nm, 0.8-1.2 μm and 4-5 μm in diameter.
9. The abrasive flow slurry for high-efficiency polishing according to claim 8, characterized in that: The mass fraction of silicon carbide abrasive grains in the slurry is 50%.
Citation Information
Cited By
Water-based two-phase flow polishing medium, polishing method and shear thinning characteristic determination method
CN120137534A
Polishing method for inner runner of high-strength aluminum alloy for additive manufacturing
CN120439192A