High-temperature-resistant suspension stabilizer for broad-spectrum well cementation working fluid as well as preparation method and application of high-temperature-resistant suspension stabilizer

By combining high-temperature salt-resistant polymers, heat-treated modified sepiolite and surface-modified inorganic nanoparticles, a broad-spectrum anti-high-temperature suspension stabilizer was prepared, which solved the problem of settlement stability of ultra-high-temperature cementing working fluid in deep wells and ultra-deep wells. , realizes the application of high temperature and high stability of cement slurry and isolation liquid systems.

CN118995159APending Publication Date: 2024-11-22CHINA NAT PETROLEUM CORP +1

Patent Information

Application Number
CN202310582341.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing technology cannot effectively respond to the settlement stability requirements of cementing working fluids in ultra-deep wells (above 200°C), and the existing suspension stabilizer functions are single, so it cannot be applied to cement slurry and isolation liquid systems at the same time.

Method used

A combination of high-temperature and salt-resistant polymers, heat-treated modified sepiolite and surface-modified inorganic nanoparticles was prepared to prepare a broad-spectrum anti-high-temperature suspension stabilizer. Through free radical solution polymerization and surface modification technology, the suspension stabilizer is enhanced. high temperature resistance.

Benefits of technology

The suspension stability of cementing working fluid system under the conditions of 120-240℃ at the bottom of the well cycle temperature was significantly improved, so that the settlement stability of cement slurry and isolation fluid system under 240℃ was controlled below 0.05g/cm3, satisfying the deep well super- Deep well cementing technology requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995159A_ABST
    Figure CN118995159A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant suspension stabilizer for a broad-spectrum well cementation working fluid as well as a preparation method and application of the high-temperature-resistant suspension stabilizer. The high-temperature-resistant suspension stabilizer comprises a high-temperature-resistant and salt-resistant polymer, heat-treatment-modified sepiolite and surface-modified inorganic nanoparticles, the high-temperature-resistant and salt-resistant polymer is a polymer prepared from 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride. The invention further discloses a preparation method of the high-temperature-resistant and salt-resistant polymer. The preparation method of the high-temperature-resistant suspension stabilizer comprises the step of uniformly mixing the high-temperature-resistant salt-resistant polymer, the heat-treatment-modified sepiolite and the surface-modified inorganic nanoparticles. The invention also provides application of the high-temperature-resistant suspension stabilizer as an additive of a well cementation working fluid system. According to the high-temperature-resistant suspension stabilizer, the suspension stability of a well cementation working fluid system at 120-240 DEG C can be improved, and the sedimentation stability of the well cementation working fluid system at 240 DEG C is controlled to be 0.05 g / cm < 3 > or below.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil and gas well cementing admixtures, and in particular relates to a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, and a preparation method and application thereof. Background Art

[0002] 39% of the remaining oil and 57% of the remaining natural gas on land are distributed in deep layers. The potential of deep and ultra-deep oil and gas resources is huge, which is of great significance to ensuring energy security. Cementing is a key technology to ensure the quality of well engineering and an important means to ensure the sustainable and high-quality development of oil and gas field exploration and development. The quality of cementing is directly related to the success or failure of drilling projects and the life of oil and gas wells. As oil and gas exploration and development advances from 7000m to 8000m and then to 9000m, the bottom hole temperature has jumped from 180℃ to above 200℃ and then to 240℃. The cementing of deep and ultra-deep wells has brought together many engineering and technical problems, the difficulty of cementing has increased, and the quality of cementing is difficult to guarantee. It poses severe challenges to high-temperature cementing working fluids such as high-temperature cementing slurry and high-temperature cementing spacer fluid and key admixtures.

[0003] Sedimentation stability is one of the important parameters to ensure the comprehensive performance of high-temperature cement slurry system and isolation fluid system, especially in ultra-high temperature cementing work in deep and ultra-deep wells. Under high temperature conditions, the thermal motion of solid phase particles in cement slurry system and isolation fluid system intensifies and is in an unbalanced state. At the same time, polymer additives are diluted at high temperature and are prone to failure, and the stability of the system cannot be guaranteed. In addition, the cementing annulus gap of deep and ultra-deep wells is small, and the stability of high-temperature cement slurry and isolation fluid is extremely high. If the cement slurry or isolation fluid is seriously unstable, it will affect the safety of cementing operations and the quality of cementing, and even worse, cause gas channeling or cementing accidents. Therefore, the development of suspension stabilizers for high-temperature and ultra-high temperature cementing working fluids and the improvement of the sedimentation stability performance of high-temperature and ultra-high temperature cementing working fluid systems are crucial to ensuring the safety of cementing operations, cementing quality and long-term effective sealing in deep and ultra-deep wells.

[0004] The prior art has disclosed relevant research on improving the suspension stability of high-temperature cementing working fluids (including cementing slurry systems and cementing spacer fluid systems). CN102086386A discloses an anti-settling agent for 200°C resistant oil well cement. The anti-settling agent is prepared by an aqueous phase free radical polymerization method using 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylamide (AM), and N-vinyl pyrrolidone (NVP), and can effectively improve the high-temperature sedimentation stability of cement slurry. The anti-settling agent was successfully tested in the cementing of three deep gas wells in Daqing Oilfield (145°C, bottom hole static temperature BHST), and the cementing quality was qualified. However, the anti-settling agent is not suitable for cementing conditions with a bottom hole circulation temperature above 200°C. Lu Haichuan (Lu Haichuan et al. Development of a new cementing suspension agent [J]. Drilling Fluids and Completion Fluids, 2014, 31(1): 60-63) used bentonite and AMPS / AM / DMAA / hydrophobic monomer copolymerized quaternary copolymer to obtain a suspension stabilizer, which has a temperature resistance of only 170°C. CN107629771A discloses a multi-branched AMPS / DMAA / AA / NVP copolymer suspension stabilizer, which has a temperature resistance of 150°C and does not thicken at low temperatures and does not dilute at high temperatures, but cannot meet the cementing requirements of deep wells and ultra-deep wells at higher temperatures. CN104962260A discloses a high-temperature isolation fluid suspension stabilizer for cementing, and its preparation method and application. The suspension stabilizer mainly comprises 58-88 parts by weight of clay, 8-20 parts by weight of wenlun gum, 0-5 parts by weight of xanthan gum, 5-10 parts by weight of inorganic salt and 2-8 parts by weight of high molecular polymer, wherein the high molecular polymer comprises one or more of polyvinyl alcohol, hydroxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl starch ether. The density of the isolation liquid system containing the suspension stabilizer is 1.10 g / cm 3 ~2.50g / cm 3 The temperature of the isolating fluid system containing the suspension stabilizer can reach 190°C.

[0005] Although the above existing technologies have achieved certain results in improving the sedimentation stability of high-temperature cement slurry or isolation fluid, they are still unable to meet the technical requirements of cementing working fluids in complex deep wells and ultra-deep wells with ultra-high temperatures (above 200°C, bottom hole circulation temperature BHCT), and their functions are relatively single and can only be applied to cement slurry systems or isolation fluid systems.

[0006] Therefore, there is an urgent need to develop a new type of high-temperature resistant suspension stabilizer for broad-spectrum cementing fluid. Summary of the invention

[0007] In order to solve the above technical problems, the purpose of the present invention is to provide a broad-spectrum high-temperature resistant suspension stabilizer for cementing working fluid and its preparation method and application. The high-temperature resistant suspension stabilizer of the present invention can improve the suspension stability of the cementing working fluid system under the condition of bottom hole circulation temperature of 120-240°C, and control the sedimentation stability of the cement slurry system and the spacer fluid system under the condition of 240°C to 0.05g / cm 3 the following.

[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, wherein the high temperature resistant suspension stabilizer comprises: a high temperature resistant and salt resistant polymer, a heat-treated modified sepiolite and surface-modified inorganic nanoparticles;

[0009] The high temperature and salt resistant polymer includes a polymer prepared by using 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N-hydroxymethyl acrylamide (HAM), N-vinyl pyrrolidone (NVP) and octadecyl dimethyl allyl ammonium chloride (DMAAC-18) as mixed monomers.

[0010] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the mass ratio of the high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles is (4.8-5.2):(1.8-2.2):(0.8-1.2), and more preferably 5:2:1.

[0011] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the molar ratio of 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride for preparing the high temperature resistant and salt resistant polymer is (10-30): (20-35): (8.5-16.5): (2-8).

[0012] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the high temperature resistant and salt resistant polymer is a polymer prepared by free radical solution polymerization of 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride as mixed monomers in the presence of an initiator.

[0013] In some specific embodiments of the present invention, preferably, the initiator includes potassium persulfate and / or ammonium persulfate, etc.

[0014] In some specific embodiments of the present invention, preferably, the amount of the initiator is 0.4-1.2% of the total mass of the mixed monomers.

[0015] In some specific embodiments of the present invention, preferably, the reaction temperature of the free radical solution polymerization is 60-80° C. and the time is 3-5 h.

[0016] In the above-mentioned high temperature resistant suspension stabilizer, more preferably, the high temperature resistant and salt resistant polymer is prepared by at least the following steps:

[0017] (1) 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N-hydroxymethyl acrylamide (HAM), N-vinyl pyrrolidone (NVP), and octadecyl dimethyl allyl ammonium chloride (DMAAC-18) are mixed and dissolved in water at a molar ratio of (10-30): (20-35): (8.5-16.5): (2-8), and the pH value is adjusted to 7-8 to obtain a mixed monomer solution;

[0018] (2) adding an initiator to the mixed monomer solution in an inert gas environment, reacting at 60 to 80° C. for 3 to 5 hours to obtain a polymer solution;

[0019] (3) The polymer solution is at least purified to obtain the high temperature and salt resistant polymer.

[0020] In some specific embodiments of the present invention, the pH adjuster used to adjust the pH value to 7-8 can be a conventional pH adjuster such as alkali solution in the art, and the present invention does not specifically limit it.

[0021] In some specific embodiments of the present invention, preferably, the total mass content of the mixed monomers in the mixed monomer solution is 20-30%.

[0022] In some specific embodiments of the present invention, preferably, the inert gas includes nitrogen or the like.

[0023] In some specific embodiments of the present invention, the initiator is added dropwise to the mixed monomer solution in the form of a solution. The concentration of the initiator solution can be conventionally adjusted by a person skilled in the art, and the present invention does not specifically limit it.

[0024] In some specific embodiments of the present invention, preferably, the purification comprises: washing the polymer solution with acetone.

[0025] In some specific embodiments of the present invention, after the polymer solution is purified, conventional drying, grinding and other steps may be performed to obtain the high temperature resistant and salt resistant polymer.

[0026] In the above-mentioned high temperature resistant suspension stabilizer, more preferably, the high temperature resistant and salt resistant polymer is in powder form, and its particle size is 200-300 meshes.

[0027] According to a specific embodiment of the present invention, from the mixed monomers used in the present invention, taking sodium hydroxide as a pH regulator as an example, it can be inferred that the reaction process for preparing the high temperature resistant and salt resistant polymer of the present invention is as follows:

[0028]

[0029] Among them, a:b:c:d=(10-30):(20-35):(8.5-16.5):(2-8), R1 and R2 respectively represent the chain segments connected by the above structural units, and the chain segments can be the same as the above structural units.

[0030] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the heat-treated modified sepiolite is prepared by at least the following steps: calcining sepiolite powder at 350-450° C. for 2-4 hours.

[0031] In some specific embodiments of the present invention, after the sepiolite powder is calcined, conventional grinding and other steps may be performed to obtain the heat-treated modified sepiolite.

[0032] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the heat-treated modified sepiolite is in powder form, and its particle size is 300-500 meshes.

[0033] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the specific surface area of ​​the heat-treated modified sepiolite is 305.84 to 426.52 m 2 / g.

[0034] According to a specific embodiment of the present invention, the crystal structure of the sepiolite used in the present invention can be as follows:

[0035]

[0036] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the surface-modified inorganic nanoparticles include inorganic nanoparticles surface-modified by a silane coupling agent. More preferably, the silane coupling agent includes one or a combination of KH-550 (γ-aminopropyltriethoxysilane), KH-792 (N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane) and KH-602 (N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane). Further preferably, the silane coupling agent is KH-550.

[0037] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the inorganic nanoparticles include one or a combination of nano-silicon dioxide, nano-titanium dioxide and nano-aluminum oxide, etc. More preferably, the inorganic nanoparticles are nano-silicon dioxide.

[0038] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the particle size of the inorganic nanoparticles which have not been surface modified is 10 to 25 nm.

[0039] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the mass ratio of the inorganic nanoparticles and the silane coupling agent in the raw material of the surface-modified inorganic nanoparticles is (1-2):(3-5).

[0040] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the surface modified inorganic nanoparticles are prepared by at least the following steps: inorganic nanoparticles and silane coupling agent in a mass ratio of (1-2): (3-5) are mixed in a solvent, and reacted at 50-60°C for 4-6 hours under stirring conditions, and then the product is subjected to at least solid-liquid separation to obtain the surface modified inorganic nanoparticles.

[0041] In some specific embodiments of the present invention, the solvent may be anhydrous ethanol.

[0042] In some specific embodiments of the present invention, after the product is separated from the solid and liquid, conventional drying, grinding and other steps may be performed to obtain the surface-modified inorganic nanoparticles.

[0043] In the above-mentioned high temperature resistant suspension stabilizer, preferably, the surface-modified inorganic nanoparticles are in powder form, and the particle size thereof is 350-400 meshes.

[0044] According to a specific embodiment of the present invention, taking KH-550 surface-modified nano-silicon dioxide as an example, the reaction process is as follows:

[0045]

[0046] The present invention has no particular limitation on the drying temperature and time, which can be routinely adjusted by those skilled in the art.

[0047] In addition, the present invention has no special limitation on the specific operation method of the above grinding, and any operation method well known in the art can be used.

[0048] The high temperature resistant suspension stabilizer of the present invention can be prepared by simply mixing the high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles.

[0049] The second aspect of the present invention provides a method for preparing the above-mentioned high temperature resistant suspension stabilizer for broad-spectrum cementing working fluid, which comprises the following steps: uniformly mixing a high temperature resistant and salt resistant polymer, a heat-treated modified sepiolite and a surface-modified inorganic nanoparticle to obtain the above-mentioned high temperature resistant suspension stabilizer for broad-spectrum cementing working fluid;

[0050] The high temperature and salt resistant polymer includes a polymer prepared by using 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N-hydroxymethyl acrylamide (HAM), N-vinyl pyrrolidone (NVP) and octadecyl dimethyl allyl ammonium chloride (DMAAC-18) as mixed monomers.

[0051] In the above preparation method, preferably, the high temperature resistant and salt resistant polymer is a polymer prepared by free radical solution polymerization of 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride as mixed monomers in a molar ratio of (10-30): (20-35): (8.5-16.5): (2-8) in the presence of an initiator.

[0052] In the above preparation method, preferably, the initiator includes potassium persulfate and / or ammonium persulfate, etc.

[0053] In the above preparation method, preferably, the amount of the initiator used is 0.4-1.2% of the total mass of the mixed monomers.

[0054] In the above preparation method, preferably, the reaction temperature of the free radical solution polymerization is 60-80° C. and the time is 3-5 h.

[0055] In the above preparation method, preferably, the heat-treated modified sepiolite is prepared by at least the following steps: calcining sepiolite powder at 350-450° C. for 2-4 hours.

[0056] In the above-mentioned preparation method, preferably, the surface-modified inorganic nanoparticles are prepared by at least the following steps: inorganic nanoparticles and silane coupling agents in a mass ratio of (1-2): (3-5) are mixed in a solvent, and reacted at 50-60°C for 4-6 hours under stirring conditions, and then the product is subjected to at least solid-liquid separation to obtain the surface-modified inorganic nanoparticles.

[0057] In the above preparation method, preferably, the silane coupling agent includes one or a combination of KH-550 (γ-aminopropyltriethoxysilane), KH-792 (N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane) and KH-602 (N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane). More preferably, the silane coupling agent is KH-550.

[0058] In the above preparation method, preferably, the inorganic nanoparticles include one or a combination of nano-silicon dioxide, nano-titanium dioxide and nano-aluminum oxide, etc. More preferably, the inorganic nanoparticles are nano-silicon dioxide.

[0059] In the above preparation method, preferably, the particle size of the inorganic nanoparticles is 10 to 25 nm.

[0060] The third aspect of the present invention provides the use of the above-mentioned high temperature resistant suspension stabilizer for broad-spectrum cementing working fluid as an additive for cementing cement slurry system and / or cementing spacer fluid system.

[0061] In the above application, preferably, based on 100 parts by weight of cement in the cementing slurry system, the added amount of the high temperature resistant suspension stabilizer is 1 to 5 parts, more preferably 1 to 2.5 parts.

[0062] In the above application, preferably, based on 100 parts by weight of water in the cementing spacer fluid system, the amount of the high temperature resistant suspension stabilizer added is 1 to 5 parts.

[0063] In the present invention, the specific formulas of the cement slurry system and the spacer fluid system can be routinely adjusted by those skilled in the art according to actual conditions, and the present invention does not specifically limit them.

[0064] In the above application, preferably, the cementing slurry system includes a special well cementing slurry system; the cementing spacer fluid system includes a special well cementing spacer fluid system. More preferably, the special wells include high temperature and high pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, and extra-deep wells.

[0065] The present invention provides a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, and a preparation method and application thereof. In the high temperature resistant and salt resistant polymer of the high temperature resistant suspension stabilizer, by introducing rigid groups and hydrophobic groups such as long branches, functional groups such as sulfonic acid, the high temperature resistant and salt resistant performance of the prepared high temperature resistant and salt resistant polymer molecular chain is improved; at the same time, by adopting N-hydroxymethyl acrylamide monomer, the polymer has a stable viscosity increasing property; furthermore, since the octadecyl dimethyl allyl ammonium chloride monomer introduces a hydrophobic group, the polymer can be intermolecularly or intramolecularly associated, and the polymer viscosity increasing performance is stably improved. The present invention obtains the high temperature resistant suspension stabilizer of the present invention by compounding the high temperature resistant and salt resistant polymer with heat-treated modified sepiolite and surface-modified inorganic nanoparticles. The high temperature resistant suspension stabilizer of the present invention has a wide applicable temperature range, can significantly improve the suspension stability of the cementing working fluid system under the condition of a bottom hole circulation temperature of 120 to 240°C, and control the sedimentation stability of the cement slurry system and the isolation fluid system under the condition of 240°C to 0.05g / cm 3 (upper and lower density difference) or less; and the raw materials of the high temperature resistant suspension stabilizer of the present invention are cheap and easily available, and have good compatibility with other cementing admixtures; and the high temperature resistant suspension stabilizer of the present invention has no adverse effects on other properties of the cement slurry system and the spacer fluid system.

[0066] Therefore, the high-temperature resistant suspension stabilizer for the broad-spectrum cementing working fluid provided by the present invention can be used to improve the suspension stability of high-temperature and ultra-high-temperature cementing cement slurry systems, and can also be used to improve the suspension stability of high-temperature and ultra-high-temperature cementing spacer fluid systems, and can meet the technical requirements of deep and ultra-deep well cementing under the condition of bottom hole circulation temperature of 120 to 240°C.

[0067] The technical solution of the present invention has at least the following beneficial effects:

[0068] (1) The high temperature resistant and salt resistant polymer in the high temperature resistant suspension stabilizer of the present invention is prepared by free radical solution polymerization, and its preparation process is simple and easy to implement. The initiator used is potassium persulfate and / or ammonium persulfate, which are inexpensive and can initiate the reaction at a relatively low temperature, with a high success rate, and can realize industrial production and large-scale promotion and application.

[0069] (2) The high temperature resistant and salt resistant polymer in the high temperature resistant suspension stabilizer of the present invention introduces rigid groups, long branched groups, sulfonic acid groups, etc., so that the high temperature resistant and salt resistant performance of the prepared high temperature resistant and salt resistant polymer molecular chain is improved; at the same time, by adopting N-hydroxymethyl acrylamide monomer, the polymer has stable viscosity-increasing properties; furthermore, since the octadecyl dimethyl allyl ammonium chloride monomer introduces hydrophobic groups, the polymer can undergo intermolecular or intramolecular association, and the polymer viscosity-increasing performance is stably improved.

[0070] (3) The high temperature resistant suspension stabilizer of the present invention includes heat-treated modified sepiolite, which is a hydrated magnesium-rich silicate clay mineral with a layered chain structure. The present invention increases its specific surface area and enhances its adsorption performance by heat-treating it, thereby improving its viscosity-increasing and temperature-resistant capabilities.

[0071] (4) The high temperature resistant suspension stabilizer of the present invention includes surface-modified inorganic nanoparticles, which have good hydrophilicity and can be well combined with the high temperature resistant and salt resistant polymer of the present invention and the heat-treated modified sepiolite to improve the heat resistance of the suspension stabilizer.

[0072] (5) The high temperature resistant suspension stabilizer of the present invention adopts a combination of three components, which makes up for the shortcomings of the existing suspension stabilizer with single material and lack of performance.

[0073] (6) The high temperature resistant suspension stabilizer of the present invention has a broad spectrum and can be used in both cement slurry system and spacer liquid system. Its viscosity and stability do not change significantly with increasing temperature and has good chemical compatibility.

[0074] (7) The applicable temperature range of the high temperature resistant suspension stabilizer of the present invention can be 120-240°C, with a wide temperature resistance range and strong adaptability, so that the sedimentation stability of the cement slurry system and the spacer liquid system at 240°C is controlled within 0.05g / cm 3 The following can meet the cementing technology requirements of special wells such as high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, and extra-deep wells. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 This is the infrared spectrum of the high temperature and salt resistance polymer prepared in Example 1.

[0076] Figure 2 ESEM images of the mixed solution with a mass concentration of 3% prepared by the high temperature resistant suspension stabilizer provided in Example 2 after thermal shearing at 25°C and 240°C. DETAILED DESCRIPTION

[0077] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0078] According to a specific embodiment of the present invention, preferably, the high temperature resistant suspension stabilizer for the broad-spectrum cementing working fluid of the present invention is prepared by at least the following steps:

[0079] A. Preparation of high temperature resistant and salt resistant polymers:

[0080] (1) 2-Acrylamido-2-methylpropanesulfonic acid (AMPS), N-hydroxymethyl acrylamide (HAM), N-vinyl pyrrolidone (NVP), octadecyl dimethyl allyl ammonium chloride (DMAAC-18) are mixed at a ratio of (10 to 30):

[0081] (20-35): (8.5-16.5): (2-8) in a molar ratio and dissolved in deionized water, and the pH value is adjusted to 7-8 with a sodium hydroxide solution to obtain a mixed monomer solution; the total mass content of the mixed monomer in the mixed monomer solution is 20-30%;

[0082] (2) introducing nitrogen into the reaction vessel to remove oxygen, adding an initiator solution dropwise using a constant pressure separatory funnel at 60 to 80° C., wherein the amount of the initiator is 0.4 to 1.2% of the total mass of the mixed monomers, and reacting at 60 to 80° C. for 3 to 5 hours to obtain a viscous liquid polymer solution; wherein the initiator includes potassium persulfate and / or ammonium persulfate;

[0083] (3) After cooling the polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 200-300 meshes to obtain a high temperature resistant and salt resistant polymer;

[0084] B. Preparation of heat-treated modified sepiolite:

[0085] The sepiolite powder is placed in a muffle furnace at 350-450°C for high temperature roasting for 2-4 hours, and then ground to 300-500 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite is 305.84-426.52 m 2 / g;

[0086] C. Preparation of surface modified inorganic nanoparticles:

[0087] Inorganic nanoparticles and silane coupling agents in a mass ratio of (1-2): (3-5) are mixed in anhydrous ethanol, ultrasonically dispersed for a period of time to improve the dispersibility and reactivity of the inorganic nanoparticles, and then reacted at 50-60° C. for 4-6 hours under stirring conditions, and then the product is centrifuged, and the obtained precipitate is dried and ground to 350-400 mesh to obtain surface-modified inorganic nanoparticles; wherein the inorganic nanoparticles are nano-silicon dioxide with a particle size of 10-25 nm; and the silane coupling agent is KH-550;

[0088] D. Preparation of high temperature resistant suspension stabilizer:

[0089] The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of (4.8-5.2):(1.8-2.2):(0.8-1.2) (preferably 5:2:1) to obtain a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid.

[0090] Example 1

[0091] This embodiment provides a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, which is prepared by the following steps:

[0092] A. Preparation of high temperature resistant and salt resistant polymers:

[0093] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of N-hydroxymethyl acrylamide, dissolve in 56 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone and 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0094] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0095] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 250 meshes to obtain a high temperature resistant and salt resistant polymer;

[0096] B. Preparation of heat-treated modified sepiolite:

[0097] The sepiolite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 400 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 350.65 m 2 / g;

[0098] C. Preparation of surface modified inorganic nanoparticles:

[0099] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0100] D. Preparation of high temperature resistant suspension stabilizer:

[0101] The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid.

[0102] Example 2

[0103] This embodiment provides a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, which is prepared by the following steps:

[0104] A. Preparation of high temperature resistant and salt resistant polymers:

[0105] (1) Weigh 19 g of 2-acrylamido-2-methylpropanesulfonic acid and 26 g of N-hydroxymethyl acrylamide, dissolve in 50 mL of deionized water, adjust the pH value to 7.8 with sodium hydroxide solution, and then dropwise add 9.56 g of N-vinyl pyrrolidone and 16.39 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0106] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.5% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 5 hours to obtain a viscous liquid polymer solution;

[0107] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 265 meshes to obtain a high temperature resistant and salt resistant polymer;

[0108] B. Preparation of heat-treated modified sepiolite:

[0109] The sepiolite powder was placed in a muffle furnace at 380°C for 2 hours and then ground to 350 mesh to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 380.63 m 2 / g;

[0110] C. Preparation of surface modified inorganic nanoparticles:

[0111] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1.5:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 5 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 380 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0112] D. Preparation of high temperature resistant suspension stabilizer:

[0113] The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid.

[0114] Example 3

[0115] This embodiment provides a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, which is prepared by the following steps:

[0116] A. Preparation of high temperature resistant and salt resistant polymers:

[0117] (1) Weigh 25 g of 2-acrylamido-2-methylpropanesulfonic acid and 27 g of N-hydroxymethyl acrylamide, dissolve them in 50 mL of deionized water, adjust the pH value to 7.5 with sodium hydroxide solution, and then dropwise add 11.35 g of N-vinyl pyrrolidone and 12.9 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0118] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.5% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 5 hours to obtain a viscous liquid polymer solution;

[0119] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 280 meshes to obtain a high temperature resistant and salt resistant polymer;

[0120] B. Preparation of heat-treated modified sepiolite:

[0121] The sepiolite powder was placed in a muffle furnace at 400°C and calcined for 3 hours, and then ground to 425 mesh to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 390.49 m 2 / g;

[0122] C. Preparation of surface modified inorganic nanoparticles:

[0123] Nano-SiO2 (particle size of 10-25nm) and silane coupling agent KH-550 were weighed in a mass ratio of 2:5 and placed in a beaker, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000r / min and a separation time of 20min; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 375 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0124] D. Preparation of high temperature resistant suspension stabilizer:

[0125] The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid.

[0126] Example 4

[0127] This embodiment provides a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, which is prepared by the following steps:

[0128] A. Preparation of high temperature resistant and salt resistant polymers:

[0129] (1) Weigh 28 g of 2-acrylamido-2-methylpropanesulfonic acid and 32 g of N-hydroxymethyl acrylamide, dissolve in 50 mL of deionized water, adjust the pH value to 7.9 with sodium hydroxide solution, and then dropwise add 13.35 g of N-vinyl pyrrolidone and 13.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0130] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.7% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 5 hours to obtain a viscous liquid polymer solution;

[0131] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 300 meshes to obtain a high temperature resistant and salt resistant polymer;

[0132] B. Preparation of heat-treated modified sepiolite:

[0133] The sepiolite powder was placed in a muffle furnace at 450°C for 4 hours and then ground to 500 mesh to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 400.86 m 2 / g;

[0134] C. Preparation of surface modified inorganic nanoparticles:

[0135] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1.5:5, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 390 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0136] D. Preparation of high temperature resistant suspension stabilizer:

[0137] The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid.

[0138] Comparative Example 1

[0139] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0140] A. Preparation of polymer:

[0141] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid, dissolve it in 40 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone and 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0142] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0143] (3) cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40 to 60° C., and grinding to 250 mesh to obtain a polymer;

[0144] B. Preparation of heat-treated modified sepiolite:

[0145] The sepiolite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 400 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 350.65 m 2 / g;

[0146] C. Preparation of surface modified inorganic nanoparticles:

[0147] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0148] D. Preparation of suspension stabilizer:

[0149] The polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a suspension stabilizer.

[0150] Comparative Example 2

[0151] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0152] A. Preparation of polymer:

[0153] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of N-hydroxymethyl acrylamide, dissolve them in 40 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone to obtain a mixed monomer solution;

[0154] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0155] (3) cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40 to 60° C., and grinding to 250 mesh to obtain a polymer;

[0156] B. Preparation of heat-treated modified sepiolite:

[0157] The sepiolite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 400 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 350.65 m 2 / g;

[0158] C. Preparation of surface modified inorganic nanoparticles:

[0159] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0160] D. Preparation of suspension stabilizer:

[0161] The polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a suspension stabilizer.

[0162] Comparative Example 3

[0163] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0164] A. Preparation of polymer:

[0165] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of acrylamide, dissolve them in 56 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0166] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0167] (3) cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40 to 60° C., and grinding to 250 mesh to obtain a polymer;

[0168] B. Preparation of heat-treated modified sepiolite:

[0169] The sepiolite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 400 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 350.65 m 2 / g;

[0170] C. Preparation of surface modified inorganic nanoparticles:

[0171] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0172] D. Preparation of suspension stabilizer:

[0173] The polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a suspension stabilizer.

[0174] Comparative Example 4

[0175] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0176] A. Preparation of high temperature resistant and salt resistant polymers:

[0177] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of N-hydroxymethyl acrylamide, dissolve in 56 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone and 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0178] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0179] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 250 meshes to obtain a high temperature resistant and salt resistant polymer;

[0180] B. Preparation of heat-treated modified sepiolite:

[0181] The sepiolite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 400 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 350.65 m 2 / g;

[0182] C. Preparation of suspension stabilizer:

[0183] The high temperature resistant and salt resistant polymer and the heat-treated modified sepiolite are uniformly mixed in a mass ratio of 5:2 to obtain a suspension stabilizer.

[0184] Comparative Example 5

[0185] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0186] A. Preparation of high temperature resistant and salt resistant polymers:

[0187] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of N-hydroxymethyl acrylamide, dissolve in 56 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone and 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0188] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0189] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 250 meshes to obtain a high temperature resistant and salt resistant polymer;

[0190] B. Preparation of surface modified inorganic nanoparticles:

[0191] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0192] C. Preparation of suspension stabilizer:

[0193] The high temperature and salt resistance polymer and the surface modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:1 to obtain a suspension stabilizer.

[0194] Comparative Example 6

[0195] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0196] A. Preparation of high temperature resistant and salt resistant polymers:

[0197] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of N-hydroxymethyl acrylamide, dissolve in 56 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone and 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0198] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0199] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 250 meshes to obtain a high temperature resistant and salt resistant polymer;

[0200] B. Preparation of heat-treated modified montmorillonite:

[0201] The montmorillonite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 300 mesh to obtain heat-treated modified montmorillonite; the specific surface area of ​​the heat-treated modified montmorillonite was 298.65 m 2 / g;

[0202] C. Preparation of surface modified inorganic nanoparticles:

[0203] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0204] D. Preparation of suspension stabilizer:

[0205] The high temperature resistant and salt resistant polymer, the heat-treated modified montmorillonite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 5:2:1 to obtain a suspension stabilizer.

[0206] Comparative Example 7

[0207] This comparative example provides a suspension stabilizer, which is prepared by the following steps:

[0208] A. Preparation of high temperature resistant and salt resistant polymers:

[0209] (1) Weigh 29 g of 2-acrylamido-2-methylpropanesulfonic acid and 20 g of N-hydroxymethyl acrylamide, dissolve in 56 mL of deionized water, adjust the pH value to 8 with sodium hydroxide solution, and then dropwise add 13.3 g of N-vinyl pyrrolidone and 14.5 g of octadecyl dimethyl allyl ammonium chloride to obtain a mixed monomer solution;

[0210] (2) nitrogen was introduced into the reaction vessel for 15 minutes to remove oxygen, and when the temperature of the reaction system rose to 80° C., a potassium persulfate solution as an initiator was added dropwise using a constant pressure separatory funnel, wherein the amount of potassium persulfate was 0.4% of the total mass of the mixed monomers. After the addition was completed in a nitrogen environment, the mixture was reacted at 80° C. for 4 hours to obtain a viscous liquid polymer solution;

[0211] (3) After cooling the viscous liquid polymer solution to room temperature, washing with acetone for purification, drying at 40-60° C., and grinding to 250 meshes to obtain a high temperature resistant and salt resistant polymer;

[0212] B. Preparation of heat-treated modified sepiolite:

[0213] The sepiolite powder was placed in a muffle furnace at 350°C for 2 hours and then ground to 400 meshes to obtain heat-treated modified sepiolite; the specific surface area of ​​the heat-treated modified sepiolite was 350.65 m 2 / g;

[0214] C. Preparation of surface modified inorganic nanoparticles:

[0215] Nano-SiO2 (particle size of 10-25 nm) and silane coupling agent KH-550 were weighed in a beaker according to a mass ratio of 1:3, and anhydrous ethanol was added as a reaction solvent; the beaker containing the rotating magnet was placed in an ultrasonic disperser for dispersion for 10 minutes; then the constant temperature magnetic stirrer was set to a moderate stirring speed and a temperature of 60°C, and the beaker was placed on the constant temperature magnetic stirrer for stirring and reacting for 6 hours; then the product was separated by a centrifuge at a speed of 4000 r / min and a separation time of 20 minutes; the separated white precipitate was placed in a beaker, heated and dried while stirring with a glass rod, and then ground to 360 meshes with a mortar to obtain surface-modified inorganic nanoparticles;

[0216] D. Preparation of suspension stabilizer:

[0217] The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed in a mass ratio of 4:3:2 to obtain a suspension stabilizer.

[0218] Test Example 1 Structural Characterization of High Temperature and Salt Resistant Polymers

[0219] In this test example, the high temperature and salt resistance polymer prepared in Example 1 was subjected to infrared spectroscopy analysis. The obtained infrared spectrum is shown in the figure below. Figure 1 shown.

[0220] The powdered high temperature resistant and salt resistant polymer prepared in Example 1 was scanned by infrared spectrum using KBr tablet method and Fourier transform infrared spectrometer with a wave number range of 4000-500 cm -1 .

[0221] Depend on Figure 1 It can be seen that the N—H stretching vibration peak in 2-acrylamide-2-methylpropanesulfonic acid monomer is located at 3472 cm -1 The C=O stretching vibration peak of the amide group and the in-plane deformation vibration peak of -NH2 are located at 1630cm -1 and 1590cm -1 1115cm -1 and 620cm -1 The peaks are the S=O and C—S absorption peaks of the sulfonic acid functional group; the stretching vibration peak of the C—N bond of the amide group in the N-vinyl pyrrolidone monomer is located at 1341 cm -13319cm -1 It is a quaternary ammonium salt—N + (CH3)2—R form characteristic peak, 2912cm -1 and 2837cm -1 They are the characteristic peaks of methyl (—CH3) and methylene (—CH2—) on the hydrophobic long chain in octadecyl dimethyl allyl ammonium chloride. The above results show that the high temperature and salt resistant polymer synthesized in Example 1 includes all the characteristic functional groups on 2-acrylamido-2-methylpropane sulfonic acid monomer, N-hydroxymethyl acrylamide monomer, N-vinyl pyrrolidone monomer and octadecyl dimethyl allyl ammonium chloride monomer. Therefore, the tetrapolymer obtained by the reaction is the target product. In addition, at 1650cm -1 -1645cm -1 There is no vibration absorption peak, which indicates that there is no C=C bond in the copolymer, indicating that the four monomers in Example 1 are fully involved in the reaction, and the high temperature and salt resistance polymer has the target design structure.

[0222] Test Example 2 ESEM Test

[0223] In this test example, the microstructure of the high temperature resistant suspension stabilizer provided in Example 2 was analyzed by environmental scanning electron microscopy (ESEM).

[0224] The high temperature resistant suspension stabilizer provided in Example 2 was mixed evenly with deionized water to prepare a mixed solution with a mass concentration of 3% of the high temperature resistant suspension stabilizer.

[0225] The mixed solution was subjected to thermal shearing at 240°C for 2 h using a Quanta 450 environmental scanning electron microscope (FEI, USA), and its microstructure before and after shearing was tested and analyzed. Figure 2 shown.

[0226] Depend on Figure 2 It can be seen from (a), (b) and (c) in Example 2 that after the high temperature resistant suspension stabilizer provided in Example 2 is mixed with deionized water, at 20°C, the high temperature resistant and salt resistant polymer therein mainly presents a multi-adsorption layer space network and film structure. Figure 2It can be seen from (d), (e) and (f) in that after thermal shearing at 240°C, some holes appeared in the high temperature and salt-resistant polymer film. Further magnification revealed that the film-like structure still existed, which indicates that high temperature will destroy the morphology of the polymer film to a certain extent. However, since the high temperature and salt-resistant polymer contains heat-resistant groups and has hydrophobic association, it can still maintain a concave plugging film association structure at high temperature. The reason for the formation of this microscopic morphology is mainly due to the mutual entanglement and curling of the molecular chains of the high temperature and salt-resistant polymer in the high temperature and salt-resistant suspension stabilizer. When the high temperature and salt-resistant suspension stabilizer comes into contact with the weighting agent, the particles in the system are adsorbed on the surface of the high temperature and salt-resistant polymer film and fill the holes between the films, thereby effectively carrying the weighting agent particles. In addition, the excellent high temperature resistance of the high temperature and salt-resistant suspension stabilizer is also attributed to the fact that the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are stable and do not decompose at high temperatures, and have the function of stable viscosity increase.

[0227] Test Example 3 Application and performance evaluation of high temperature resistant suspension stabilizer for broad-spectrum cementing fluid

[0228] This test example tests the sedimentation stability performance of the spacer liquid system and cement slurry system prepared with the suspension stabilizer provided in Examples 1 to 4 and Comparative Examples 1 to 7, respectively.

[0229] 1. Evaluation of sedimentation stability of high temperature and ultra-high temperature isolation fluid system

[0230] The isolation liquid system of this test example is prepared by the following steps: weigh 100 parts by weight of water in a slurry cup, slowly add 1 to 5 parts by weight of the suspension stabilizer sample into the water, stir at a speed of 1500 to 2500 r / min for 20 minutes on a high-speed stirrer, add weighting material according to the required density of the isolation liquid system after stirring evenly, and then stir at a speed of 1500 to 2000 r / min for 25 minutes, then add 0.1 to 0.2 parts by weight of glycerol polyoxypropylene ether defoamer to the system, stir at a speed of 200 to 300 r / min for 1 minute, and let it stand for use. Among them, the weighting material is barite (4.30 g / cm 3 ).

[0231] The suspension stabilizers provided in the examples and comparative examples were prepared to have a density of 1.50 g / cm 3 , 2.30g / cm 3 Isolation fluid system.

[0232] 1.50g / cm 3 The formula of the isolation liquid system is: 100 parts by weight of water + 85 parts by weight of barite + 3 parts by weight of suspension stabilizer + 0.1-0.2 parts by weight of glycerol polyoxypropylene ether defoamer;

[0233] 2.30g / cm3 The formula of the isolation liquid system is: 100 parts by weight of water + 320 parts by weight of barite + 3 parts by weight of suspension stabilizer + 0.1-0.2 parts by weight of glycerol polyoxypropylene ether defoamer.

[0234] According to the method described in the standard GB / T 1884-2000 "Laboratory Determination of Density of Crude Oil and Liquid Petroleum Products (Densitometer Method)", the sedimentation stability of the above-mentioned spacer liquid system at 120-240°C was tested. The test results are shown in Tables 1-3.

[0235] Table 1 shows the sedimentation stability of the isolation liquid system prepared by using the suspension stabilizers provided in the examples and comparative examples at 120°C. It can be seen from Table 1 that the 1.50 g / cm 3 The upper and lower density difference of the isolation liquid system is 0, and the plastic viscosity is 45-50 mPa·s; the 1.50 g / cm 3 The upper and lower density difference of the isolation liquid system is 0.014~0.039g / cm 3 , plastic viscosity is 33-41 mPa·s; 2.30 g / cm prepared by the suspension stabilizer provided in Examples 1-4 3 The density difference between the upper and lower parts of the isolation liquid system is less than 0.03g / cm 3 , compared with comparative examples 1 to 7, it has better suspension stability.

[0236] Table 1 Sedimentation stability of the spacer liquid system at 120℃

[0237]

[0238] Table 2 shows the sedimentation stability of the isolation liquid system prepared by using the suspension stabilizers provided in the examples and comparative examples at 180°C. It can be seen from Table 2 that the 1.50 g / cm 3 The density difference between the upper and lower parts of the isolation liquid system is 0.03g / cm 3 The following; using the suspension stabilizer prepared by Comparative Examples 1 to 7 1.50g / cm 3 The upper and lower density difference of the isolation liquid system is 0.045~0.075g / cm 3 ; 2.30g / cm prepared by the suspension stabilizer provided in Examples 1 to 4 3 The density difference between the upper and lower parts of the isolation liquid system is less than 0.04g / cm 3 , compared with comparative examples 1 to 7, it has better suspension stability.

[0239] Table 2 Sedimentation stability of the spacer liquid system at 180℃

[0240]

[0241]

[0242] Table 3 shows the sedimentation stability of the isolation liquid system prepared by the suspension stabilizers provided in the examples and comparative examples at 240°C. The higher the temperature, the worse the sedimentation stability of the isolation liquid system. It can be seen from Table 3 that the 1.50 g / cm 3 and 2.30g / cm 3 The upper and lower density differences of the isolation liquid system are both less than 0.05g / cm 3 , 1.50g / cm prepared by the suspension stabilizer provided in Comparative Examples 1 to 7 3 and 2.30g / cm 3 The upper and lower density difference of the isolation liquid system is 0.160~0.403g / cm 3 Compared with the suspension stabilizer in the comparative example, the isolation liquid system prepared with the suspension stabilizer provided in the embodiment has better suspension stability.

[0243] Table 3 Sedimentation stability of the spacer liquid system at 240℃

[0244]

[0245] 2. Evaluation of sedimentation stability of high temperature and ultra-high temperature cement slurry system

[0246] In this test example, the formula of the cement slurry system tested at 120°C is: 100 parts by weight of Jiahua G-grade oil well cement (high sulfur resistance, HSR) + 25 parts by weight of quartz sand (200 mesh) + 2 parts by weight of microsilicon + 1 part by weight of dispersant + 1.8 parts by weight of retarder + 3 parts by weight of liquid fluid loss additive + 1 part by weight of suspension stabilizer + 48 parts by weight of water; the density of the cement slurry system is 1.85 g / cm 3 .

[0247] The formula of the cement slurry system tested at 180°C is: 100 parts by weight of Jiahua G-grade oil well cement (high sulfur resistance, HSR) + 25 parts by weight of quartz sand (200 mesh) + 15 parts by weight of quartz sand (600 mesh) + 1 part by weight of microsilicon + 1 part by weight of dispersant + 3 parts by weight of retarder + 3.8 parts by weight of liquid fluid loss agent + 1.5 parts by weight of suspension stabilizer + 50 parts by weight of water; the density of the cement slurry system is 1.85 g / cm 3 .

[0248] The formula of the cement slurry system tested at 240°C is: 100 parts by weight of Jiahua G-grade oil well cement (high sulfur resistance, HSR) + 40 parts by weight of silica sand + 1 part by weight of dispersant + 4 parts by weight of retarder + 2 parts by weight of liquid fluid loss additive + 2.5 parts by weight of suspension stabilizer + 38 parts by weight of water; the density of the cement slurry system is 1.85 g / cm 3 .

[0249] Among them, the dispersant, retarder and liquid fluid loss reducer are aldehyde-ketone condensation polymer dispersant DRS-1S, acrylamide retarder DRH-3L and acrylamide fluid loss reducer DRF-2L, all of which are products produced by China National Petroleum Corporation Engineering and Technology Research Institute Co., Ltd.

[0250] The performance of the cement slurry system prepared with the suspension stabilizer provided in Examples 1 to 4 and Comparative Examples 1 to 7 was evaluated according to the method described in the petroleum and natural gas industry standard GB / T 19139-2012 "Test Methods for Oil Well Cement", and the results are shown in Tables 4 to 6.

[0251] Among them, the sedimentation stability of the cement slurry system was investigated by the following methods:

[0252] Method 1: The cement slurry system is passed through a high-temperature and high-pressure thickener and cured at high temperature (including 120°C, 180°C and 240°C) for 30 minutes, then cooled to 90°C, removed, the surface oil removed, stirred evenly and placed at 90°C for 2 hours, then the density difference between the upper and lower parts of the cement slurry system is tested, and the amount of free liquid is examined at the same time.

[0253] Method 2: In order to simulate the change of the settlement stability of the cement slurry system when the pumping is stopped due to unexpected circumstances during the ultra-high temperature cementing operation in deep wells and ultra-deep wells, the instantaneous viscosity change value of the cement slurry system after being stopped for 30 minutes under high temperature (including 120℃, 180℃ and 240℃) conditions was investigated to study its settlement stability performance; if the instantaneous viscosity recoil value of the startup is greater than 40BC, the fluid pumping pressure will be greatly increased, and there is a risk of leakage of the formation; if it is less than 40BC, the settlement stability of the cement slurry system is considered to be good.

[0254] This test example investigates the improvement effect of the suspension stabilizer on the sedimentation stability of the cement slurry system by combining the above methods.

[0255] As shown in Table 4, the cement slurry systems added with the suspension stabilizers provided in Examples 1 to 4 at 120°C have good sedimentation stability, the ash removal time is less than 30s, and the sedimentation stability is controlled at 0.02g / cm 3(upper and lower density difference) below, there is no free liquid, and the suspension is normal; however, the cement slurry system with the suspension stabilizer provided in Comparative Examples 1 to 7 respectively has a relatively long ash-down time and poor sedimentation stability (upper and lower density difference is 0.03g / cm 3 The free liquid is more than 0.8%, and the instantaneous viscosity rebound is high after the machine is stopped for 30 minutes. Therefore, the comprehensive performance of the cement slurry system prepared with the suspension stabilizer provided in the embodiment at 120°C is better than that of the comparative example.

[0256] Table 4 Sedimentation stability of cement slurry system at 120℃

[0257]

[0258]

[0259] Note: # represents the weight percentage of cement; experimental conditions: temperature 120℃, pressure 45MPa, heating time 45min.

[0260] As shown in Table 5, the cement slurry system containing the suspension stabilizers provided in Examples 1 to 4 at 180°C has good sedimentation stability, the ash removal time is less than 35s, and the sedimentation stability is controlled at 0.04g / cm 3 Below, there is no free liquid, and the suspension is normal; however, the cement slurry system with the suspension stabilizer provided in Comparative Examples 1 to 7 has a relatively long ash-down time and poor sedimentation stability (the upper and lower density difference is 0.05 to 0.15 g / cm 3 ), more free liquid (more than 1%), and the instantaneous viscosity rebound is high after the machine is stopped for 30 minutes. Therefore, the comprehensive performance of the cement slurry system prepared with the suspension stabilizer provided in the embodiment at 180°C is better than that of the comparative example.

[0261] Table 5 Sedimentation stability of cement slurry system at 180℃

[0262]

[0263] Note: # represents the weight percentage of cement; experimental conditions: temperature 180℃, pressure 70MPa, heating time 70min.

[0264] It can be seen from Table 6 that the cement slurry system added with the suspension stabilizers provided in Examples 1 to 4 at 240°C has good sedimentation stability, the ash removal time is less than 40s, and the sedimentation stability is controlled at 0.05g / cm 3 Below, there is no free liquid, and the suspension is normal; however, the cement slurry system with the suspension stabilizer provided in Comparative Examples 1 to 7 is difficult to ash, and the sedimentation stability is poor (the upper and lower density difference is greater than 0.1g / cm 3), more free liquid (more than 2%), and the instantaneous viscosity rebound is high after the machine is stopped for 30 minutes. Therefore, the comprehensive performance of the cement slurry system prepared with the suspension stabilizer provided in the embodiment at 240°C is better than that of the comparative example.

[0265] Table 6 Sedimentation stability of cement slurry system at 240℃

[0266]

[0267] Note: # represents the weight percentage of cement; experimental conditions: temperature 240℃, pressure 160MPa, heating time 130min.

[0268] In summary, the high-temperature resistant suspension stabilizer for the broad-spectrum cementing working fluid provided by the present invention is beneficial to improving the suspension stability of the cementing isolation fluid system and the cementing cement slurry system under high-temperature and ultra-high-temperature conditions, and can ensure the comprehensive performance of the cementing working fluid system under high-temperature and ultra-high-temperature conditions and the safety of cementing operations, and has good application prospects in cementing operations in deep wells, ultra-deep wells, extra-deep wells, high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, etc.

Claims

1. A high temperature resistant suspension stabilizer for a broad-spectrum cementing working fluid, the high temperature resistant suspension stabilizer comprising: High temperature and salt resistant polymers, thermally modified sepiolite, and surface modified inorganic nanoparticles; The high temperature and salt resistant polymer comprises a polymer prepared by using 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride as mixed monomers.

2. The high temperature resistant suspension stabilizer according to claim 1, wherein: The mass ratio of the high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles is (4.8-5.2):(1.8-2.2):(0.8-1.2), preferably 5:2:

1.

3. The high temperature resistant suspension stabilizer according to claim 1, wherein: The molar ratio of 2-acrylamide-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride for preparing the high temperature resistant and salt resistant polymer is (10-30): (20-35): (8.5-16.5): (2-8).

4. The high temperature resistant suspension stabilizer according to claim 1, wherein: The high temperature and salt resistant polymer is a polymer prepared by free radical solution polymerization of 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride as mixed monomers in the presence of an initiator; Preferably, the initiator comprises potassium persulfate and / or ammonium persulfate; Preferably, the amount of the initiator is 0.4 to 1.2% of the total mass of the mixed monomers; Preferably, the reaction temperature of the free radical solution polymerization is 60-80° C. and the reaction time is 3-5 hours.

5. The high temperature resistant suspension stabilizer according to claim 4, wherein: The high temperature resistant and salt resistant polymer is prepared by at least the following steps: (1) 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone, and octadecyl dimethyl allyl ammonium chloride are mixed in a molar ratio of (10-30): (20-35): (8.5-16.5): (2-8) and dissolved in water, and the pH value is adjusted to 7-8 to obtain a mixed monomer solution; (2) adding an initiator to the mixed monomer solution in an inert gas environment, reacting at 60 to 80° C. for 3 to 5 hours to obtain a polymer solution; (3) Purifying the polymer solution to obtain the high temperature resistant and salt resistant polymer; Wherein, preferably, the total mass content of the mixed monomers in the mixed monomer solution is 20-30%; Preferably, the inert gas comprises nitrogen; Preferably, the purification comprises: washing the polymer solution with acetone.

6. The high temperature resistant suspension stabilizer according to any one of claims 1 to 5, wherein The high temperature resistant and salt resistant polymer is in powder form, and its particle size is 200-300 meshes.

7. The high temperature resistant suspension stabilizer according to claim 1, wherein: The heat-treated modified sepiolite is prepared by at least the following steps: calcining sepiolite powder at 350-450° C. for 2-4 hours.

8. The high temperature resistant suspension stabilizer according to any one of claims 1, 2 and 7, wherein The heat-treated modified sepiolite is in powder form, and its particle size is 300-500 meshes; Preferably, the specific surface area of ​​the heat-treated modified sepiolite is 305.84 to 426.52 m 2 / g.

9. The high temperature resistant suspension stabilizer according to claim 1, wherein: The surface-modified inorganic nanoparticles include inorganic nanoparticles whose surfaces are modified by a silane coupling agent.

10. The high temperature resistant suspension stabilizer according to claim 9, wherein: The silane coupling agent includes one or a combination of KH-550, KH-792 and KH-602; Preferably, the silane coupling agent is KH-550.

11. The high temperature resistant suspension stabilizer according to claim 9, wherein: The inorganic nanoparticles include one or a combination of nano silicon dioxide, nano titanium dioxide and nano aluminum oxide; Preferably, the inorganic nanoparticles are nano-silicon dioxide; Preferably, the particle size of the inorganic nanoparticles that have not been surface-modified is 10 to 25 nm.

12. The high temperature resistant suspension stabilizer according to claim 9, wherein: The mass ratio of the inorganic nanoparticles to the silane coupling agent in the raw materials of the surface-modified inorganic nanoparticles is (1-2):(3-5).

13. The high temperature resistant suspension stabilizer according to claim 9, wherein: The surface-modified inorganic nanoparticles are prepared by at least the following steps: mixing inorganic nanoparticles and a silane coupling agent in a mass ratio of (1-2):(3-5) in a solvent, reacting at 50-60° C. for 4-6 hours under stirring conditions, and then subjecting the product to at least solid-liquid separation to obtain the surface-modified inorganic nanoparticles.

14. The high temperature resistant suspension stabilizer according to any one of claims 1, 2, 9 and 13, wherein The surface-modified inorganic nanoparticles are in powder form, and the particle size thereof is 350-400 meshes.

15. A method for preparing the high temperature resistant suspension stabilizer for broad-spectrum cementing working fluid according to any one of claims 1 to 14, comprising the following steps: The high temperature resistant and salt resistant polymer, the heat-treated modified sepiolite and the surface-modified inorganic nanoparticles are uniformly mixed to obtain the high temperature resistant suspension stabilizer for the broad-spectrum cementing working fluid; The high temperature and salt resistant polymer comprises a polymer prepared by using 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride as mixed monomers.

16. The preparation method according to claim 15, wherein: The high temperature and salt resistant polymer is a polymer prepared by free radical solution polymerization of 2-acrylamido-2-methylpropanesulfonic acid, N-hydroxymethyl acrylamide, N-vinyl pyrrolidone and octadecyl dimethyl allyl ammonium chloride as mixed monomers in a molar ratio of (10-30): (20-35): (8.5-16.5): (2-8) in the presence of an initiator; Preferably, the initiator comprises potassium persulfate and / or ammonium persulfate; Preferably, the amount of the initiator is 0.4 to 1.2% of the total mass of the mixed monomers; Preferably, the reaction temperature of the free radical solution polymerization is 60-80° C. and the reaction time is 3-5 hours.

17. The preparation method according to claim 15, wherein: The heat-treated modified sepiolite is prepared by at least the following steps: calcining sepiolite powder at 350-450° C. for 2-4 hours.

18. The preparation method according to claim 15, wherein: The surface-modified inorganic nanoparticles are prepared by at least the following steps: mixing inorganic nanoparticles and a silane coupling agent in a mass ratio of (1-2):(3-5) in a solvent, reacting at 50-60° C. for 4-6 hours under stirring conditions, and then subjecting the product to at least solid-liquid separation to obtain the surface-modified inorganic nanoparticles; Preferably, the silane coupling agent includes one or a combination of KH-550, KH-792 and KH-602; more preferably, the silane coupling agent is KH-550; Preferably, the inorganic nanoparticles include one or a combination of nano-silicon dioxide, nano-titanium dioxide and nano-aluminum oxide; more preferably, the inorganic nanoparticles are nano-silicon dioxide; Preferably, the particle size of the inorganic nanoparticles is 10 to 25 nm.

19. Use of the high temperature resistant suspension stabilizer for broad-spectrum cementing working fluid according to any one of claims 1 to 14 as an additive for cementing slurry system and / or cementing spacer fluid system.

20. The use according to claim 19, wherein: Based on 100 parts by weight of cement in the cementing slurry system, the amount of the high temperature resistant suspension stabilizer added is 1 to 5 parts; Preferably, the amount of the high temperature resistant suspension stabilizer added is 1 to 5 parts based on 100 parts by weight of water in the cementing spacer fluid system; Preferably, the cementing cement slurry system includes a special well cementing cement slurry system, and the cementing spacer fluid system includes a special well cementing spacer fluid system; more preferably, the special wells include high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, and extra-deep wells.

Citation Information

Patent Citations

  • Anti-sedimentation agent for cement capable of resisting 200 DEG C of oil well and preparation method thereof

    CN102086386A

  • High-temperature spacer fluid suspension stabilizer for well cementation, preparation method of high-temperature spacer fluid suspension stabilizer and application of high-temperature spacer fluid suspension stabilizer

    CN104962260A

  • High temperature-resistant insulating fluid suspension stabilizer

    CN107177350A

  • Preparation method of low viscosity and high shear oil well cement suspension stabilizer for large temperature difference well cementation

    CN107629771A

Cited By

  • High-temperature-resistant workover fluid and preparation method thereof

    CN121852010A

  • High temperature resistant workover fluid and method of making same

    CN121852010B

  • Broad-spectrum anti-pollution spacer fluid for ultra-deep well cementation and preparation method of broad-spectrum anti-pollution spacer fluid

    CN122302849A

  • High-temperature-resistant suspending stabilizer for water-based high-fluid-loss leak-stopping slurry, preparation method and application thereof

    CN122749811A

  • A reservoir protection agent for oil and gas fields, a preparation method and application thereof

    CN122750331A