Method for comprehensively utilizing lepidolite
By combining low-temperature leaching with nanofiltration, nanofiltration cation separation, and bipolar membrane electrodialysis, the problems of high energy consumption and loss of valuable metals in the leaching process of lepidolite concentrate have been solved, achieving efficient and environmentally friendly utilization of lepidolite resources.
Patent Information
- Application Number
- CN202411136295.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Existing leaching processes for lepidolite concentrate are energy-intensive, generate fluorine-containing waste gas and wastewater, and result in significant loss of valuable metals in lepidolite, leading to high production costs.
By employing technologies such as low-temperature leaching combined with nanofiltration, nanofiltration cation separation, high-pressure nanofiltration concentration, and bipolar membrane electrodialysis, valuable metals such as lithium, rubidium, and cesium are separated and recovered, fluorine-containing waste is recycled, and energy consumption and metal loss are reduced.
This method achieves efficient leaching of lepidolite, reduces energy consumption, minimizes the loss of valuable metals, avoids the emission of fluorine-containing wastewater and exhaust gas, and improves production efficiency and economic benefits.
Smart Images

Figure CN118996154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ore recovery and utilization, and in particular relates to a method for comprehensive utilization of lepidolite. Background Art
[0002] As the target deadlines for carbon peak and carbon neutrality in various countries approach, global environmental emission standards will become more stringent. The large amount of carbon emissions generated by traditional fossil fuel vehicles and thermal power generation will be difficult to meet environmental protection requirements. The power and energy industry is facing the pressure of transforming to a new clean and energy-saving industry. Therefore, the power battery and lithium battery energy storage system industries have developed rapidly in recent years, resulting in a continuous increase in demand for lithium and its compounds, the key raw materials for lithium batteries.
[0003] Natural lithium resources include lithium-containing salt lakes and lithium ores. The advantage of lithium extraction from lithium-containing salt lakes is that the production cost is relatively low, but there are corresponding problems such as high requirements for lithium extraction technology, large differences in water quality between different salt lakes, large initial investment, long cost recovery period, and higher environmental protection requirements for mining due to the fragility of the natural environment of salt lakes. Compared with salt lake lithium, ore lithium has the advantages of high grade and simple composition. After separation and enrichment, it is easier to meet product standards. The disadvantage is that the mining and production cost is relatively high. Lithium ore is mainly divided into two types of deposits: spodumene and lepidolite. Spodumene has a simple elemental composition and high lithium grade. my country has abundant reserves, but the high-altitude and cold mining environment limits its industrial development and utilization to a certain extent. Lepidolite resources are abundant and the difficulty of mining is relatively low. Unlike spodumene, lepidolite has a low lithium grade, complex chemical composition and fluorine, and is accompanied by rubidium and cesium. The fluorine element will cause lithium loss during the lithium extraction process, affecting the leaching of lithium, and will become a pollutant if it is directly discharged or discarded. Rubidium and cesium elements are of high value and require supporting recycling processes to increase production returns and make up for the high production cost of lithium extraction from lithium mica.
[0004] The existing leaching processes for lithium mica concentrate are mainly sulfuric acid method and sulfate method. The sulfuric acid method involves crushing the lithium mica concentrate and then roasting it in high-temperature steam above 870°C for defluorination. Then, it is mixed with concentrated sulfuric acid and roasted at 300-450°C to leach lithium and other metal elements. After the leachate is impurized, lithium carbonate, rubidium sulfate and cesium sulfate solutions are produced. The sulfate method requires adding sulfate after the concentrate is crushed and roasting at 900°C to convert the mica into soluble sulfate, and then leaching the metal elements with dilute sulfuric acid. The subsequent process is similar to the sulfuric acid method. The above processes inevitably have extremely high leaching energy consumption and produce fluorine-containing waste gas and wastewater to be treated. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the related art. To this end, the present invention proposes a method for comprehensive utilization of lepidolite, which can achieve efficient leaching of lepidolite, reduce energy consumption and metal loss, and recycle fluorine-containing waste materials to comprehensively produce lithium, aluminum, rubidium, cesium and other metals with high recovery value, so as to solve the problems inherent in the above process, such as high production cost, wastewater generation, hazardous waste to be treated, etc.
[0006] The above technical objectives of the present invention are achieved through the following technical solutions:
[0007] A method for comprehensive utilization of lepidolite comprises the following steps:
[0008] (1) mixing lepidolite ore powder with leaching acid, leaching, and filtering to obtain a leachate and a leaching residue;
[0009] (2) subjecting the leaching solution obtained in step (1) to nanofiltration acid purification, nanofiltration cation separation and high-pressure nanofiltration concentration in sequence to obtain high-pressure nanofiltration fresh water and high-pressure nanofiltration concentrated water, and subjecting the high-pressure nanofiltration concentrated water to electrodialysis to obtain electrodialysis acid solution and electrodialysis alkali solution;
[0010] (3) evaporating and concentrating the electrodialysis alkali solution obtained in step (2) and then cooling and crystallizing it, filtering to obtain lithium hydroxide monohydrate crystals and a crystallization mother liquor, introducing carbon dioxide into the crystallization mother liquor, and filtering to obtain lithium carbonate and lithium precipitation mother liquor after the reaction;
[0011] (4) extracting the lithium precipitated mother liquor obtained in step (3) to separate a loaded organic phase and a raffinate, stripping the loaded organic phase with a stripping acid to obtain a stripping solution A and a preliminary stripping organic phase, further stripping the preliminary stripping organic phase with a stripping acid to obtain a stripping solution B, evaporating and crystallizing the stripping solution A to produce a rubidium salt, and evaporating and crystallizing the stripping solution B to produce a cesium salt;
[0012] (5) The pH of the metal cation concentrated aqueous solution produced in the nanofiltration cation separation process is adjusted to 6.0-7.0, and potassium fluorosilicate and a filtrate are obtained by filtering, and the pH of the filtrate is further adjusted to alkaline, and aluminum hydroxide and aluminum precipitation mother liquor are obtained by filtering.
[0013] In one embodiment, the invention further comprises the following steps: evaporating the aluminum precipitation mother liquor obtained in step (5) until the aluminum precipitation mother liquor is saturated with sodium salt, and then separating the sodium salt and potassium salt by a stepwise freezing crystallization process.
[0014] In one embodiment, the invention further comprises the following steps: collecting distilled water produced by evaporation and concentration of the electrodialysis alkali solution, evaporation and crystallization of the stripping solution A, evaporation and crystallization of the stripping solution B, and evaporation of the aluminum precipitation mother solution, and using the distilled water to dilute the leaching solution in step (1).
[0015] In one embodiment, the invention further comprises the following steps: performing acid concentration on at least one of the nanofiltration acid purified fresh water solution produced by the nanofiltration acid purification, the high-pressure nanofiltration fresh water, the electrodialysis acid solution and the acidic washing water obtained after washing the leaching residue for use in preparing the leaching acid in step (1).
[0016] In one embodiment, the acid concentration refers to concentrating the acidic wastewater using one of a reverse osmosis concentration process, a low-temperature evaporation concentration process, and a falling film evaporation concentration process to obtain H + The concentrated acid has a molar concentration of 6-8 mol / L. The acidic wastewater is at least one of the nanofiltration acid purified fresh water, the high-pressure nanofiltration fresh water, the electrodialysis acid solution and the acidic wash water obtained after washing the leaching residue.
[0017] In one embodiment, in step (1), the leaching acid is a mixture of fluorosilicic acid and other inorganic acids, and the other inorganic acids include at least one of hydrochloric acid, sulfuric acid and phosphoric acid.
[0018] In one embodiment, the mass ratio of the leaching acid to the lithium mica ore powder is (2-5):1, and the leaching acid needs to be supplemented with other inorganic acids in each cycle, and the supplementary amount is determined by the amount of other metal elements (mainly including potassium, sodium, rubidium, and cesium elements) in the lithium mica ore powder except lithium and aluminum elements, and the supplementary amount is calculated according to 90%-200%wt of the theoretical amount required for the anions in the other inorganic acids to completely combine with the ions of the other metal elements.
[0019] In one embodiment, in step (1), the leaching temperature is 80-150° C., the pressure is 0.1-1.0 MPa, and the reaction time is 1-4 hours.
[0020] In one embodiment, in step (1), the leachate contains H + The molar concentration is 4-6 mol / L.
[0021] In one embodiment, in step (1), the leached residue is used as a raw material for producing building materials after washing, and acidic washing water is generated. The main components of the leached residue are silicon dioxide and a small amount of aluminosilicate (such as sodium aluminosilicate) or fluorosilicate (such as sodium fluorosilicate), and silicon phosphate, which are used as raw materials for building materials such as glass, ceramics, and concrete.
[0022] In one embodiment, in step (2), the nanofiltration acid purification is to perform acid purification on the leachate through a nanofiltration membrane to obtain a nanofiltration acid-purified concentrated water solution and a nanofiltration acid-purified fresh water solution, and the nanofiltration acid-purified concentrated water solution enters the nanofiltration cation separation step.
[0023] In one embodiment, the nanofiltration acid purification adopts multi-stage acid-resistant nanofiltration membrane purification, and the typical operating environment of the acid-resistant nanofiltration membrane in the nanofiltration acid purification is: sulfuric acid solution or hydrochloric acid solution below 20wt%, phosphoric acid solution below 30wt%, the number of series stages is 3-7, and the pressure before the membrane is 1.0-1.5MPa.
[0024] In one embodiment, in step (2), the nanofiltration cation separation is to perform cation separation treatment on the nanofiltration acid purified concentrated water solution through a nanofiltration membrane to obtain a metal cation fresh water solution and the metal cation concentrated water solution, and the metal cation fresh water solution enters the high-pressure nanofiltration concentration step.
[0025] In one embodiment, in step (2), the metal cations in the metal cation fresh water solution are monovalent metal cations, and the metal cation fresh water solution contains potassium ions, lithium ions, sodium ions, rubidium ions and cesium ions; the metal cations in the metal cation concentrated water solution are high-valent metal cations, and the metal cation concentrated water solution contains aluminum ions.
[0026] In one embodiment, the nanofiltration cation separation uses multi-stage acid-resistant nanofiltration membrane concentration, the number of series stages is 3-7, and the pressure before the membrane is 1.5-2.5 MPa.
[0027] In one embodiment, in step (2), the high-pressure nanofiltration concentration is to concentrate the metal cation fresh water solution through a nanofiltration membrane to obtain the high-pressure nanofiltration fresh water and the high-pressure nanofiltration concentrated water.
[0028] In one embodiment, the high-pressure nanofiltration concentration uses multi-stage acid-resistant nanofiltration membrane concentration, the number of series stages is 3-7, and the pressure before the membrane is 3-6 MPa.
[0029] In one embodiment, in step (2), the electrodialysis is a bipolar membrane electrodialysis, and the electrodialysis device used comprises a stock solution chamber, an electrodialysis alkali solution chamber and an electrodialysis acid solution chamber, the electrodialysis alkali solution chamber and the stock solution chamber are separated by a cationic membrane, and the electrodialysis acid solution chamber and the stock solution chamber are separated by an anionic membrane, the electrodes of the bipolar membrane electrodialysis device are titanium-plated ruthenium-iridium electrodes, and the electrode liquid is a lithium hydroxide solution with a mass percentage concentration of 1%-4%.
[0030] In one embodiment, during the bipolar membrane electrodialysis, OH in the electrodialysis alkali solution chamber - When the concentration rises to 1.8-2.2 mol / L, the alkali solution is discharged.
[0031] In one embodiment, in step (3), the electrodialysis alkali solution is evaporated and concentrated until the potassium hydroxide component therein is saturated at room temperature, and then cooled and crystallized.
[0032] In one embodiment, in step (3), the temperature of the cooling crystallization is 10-30°C.
[0033] In one embodiment, in step (3), before the evaporation concentration, the electrodialysis alkali solution is concentrated by using an alkali-resistant high-pressure reverse osmosis membrane until the Li content therein reaches 32-37 g / L.
[0034] In one embodiment, in step (3), the lithium hydroxide monohydrate is washed and dried to obtain battery-grade lithium hydroxide monohydrate.
[0035] In one embodiment, in step (3), the lithium carbonate is washed and dried to obtain a battery-grade lithium carbonate product.
[0036] In one embodiment, in step (4), the stripping solution A and the stripping solution B are both subjected to oil removal pretreatment before evaporation and crystallization so that the oil in the stripping solution A and the stripping solution B is reduced to below 5 mg / L.
[0037] In one embodiment, in step (4), the raffinate is pretreated to remove oil so that the oil in the raffinate is reduced to below 5 mg / L.
[0038] In one embodiment, in step (5), the adjusting agent used to adjust the pH is at least one of KOH, NaOH and the raffinate.
[0039] In one embodiment, in step (5), adjusting the pH of the filtrate to alkaline means adjusting the pH to 8.0-9.0.
[0040] In one embodiment, in step (5), the aluminum precipitation mother liquor is pre-treated with a heavy metal removal resin to remove impurities, and the potassium salt obtained by crystallization can be sold as potash fertilizer.
[0041] In one embodiment, in step (5), the aluminum precipitation mother liquor is directly evaporated to dryness, and potassium salt containing a small amount of sodium salt is produced and sold as potash fertilizer.
[0042] In one embodiment, a method for comprehensive utilization of lepidolite comprises the following steps:
[0043] S1. Leaching: adding leaching acid to the lithium mica ore powder for low-temperature reaction, cooling to room temperature after the reaction, adding distilled water to dilute the leaching, filtering and separating to obtain the leachate and the leach residue;
[0044] S2. Nanofiltration acid purification: The leachate is subjected to acid purification using a nanofiltration membrane to obtain a nanofiltration acid-purified concentrated water solution and a nanofiltration acid-purified fresh water solution;
[0045] S3. Nanofiltration cation separation: The nanofiltration acid-purified concentrated water solution is treated with a nanofiltration membrane for cation separation to obtain a metal cation desalted water solution and a metal cation concentrated water solution;
[0046] S4. High-pressure nanofiltration concentration and bipolar membrane electrodialysis: The metal cation freshwater solution is concentrated by a high-pressure nanofiltration membrane to obtain high-pressure nanofiltration freshwater and high-pressure nanofiltration concentrated water, and the high-pressure nanofiltration concentrated water is subjected to bipolar membrane electrodialysis to obtain electrodialysis acid and electrodialysis alkali solution;
[0047] S5. Evaporation concentration and cooling crystallization: The electrodialysis alkali solution is treated by evaporation concentration process until the potassium hydroxide component is saturated at room temperature, and then cooled and crystallized, and filtered to obtain lithium hydroxide monohydrate crystals and crystallization mother liquor;
[0048] S6. Carbonization of lithium precipitate: carbon dioxide is introduced into the crystallization mother liquor to generate a precipitate and filter to obtain lithium carbonate and lithium precipitate mother liquor;
[0049] S7. Multi-stage extraction and separation, stripping: The lithium precipitation mother liquor is treated by a multi-stage extraction and separation process to obtain a loaded organic phase and a raffinate, the loaded organic phase is stripped with a stripping acid to obtain a stripping solution A and a preliminary stripping organic phase, the preliminary stripping organic phase is further stripped with a stripping acid to obtain a stripping solution B, and the raffinate, stripping solution A, and stripping solution B are pretreated for oil removal;
[0050] S8. Evaporation and crystallization: evaporating and crystallizing the stripping solution A to produce a rubidium salt, and evaporating and crystallizing the stripping solution B to produce a cesium salt;
[0051] S9. Fluoride removal and aluminum precipitation: using a pH adjusting agent to adjust the pH of the metal cation concentrated aqueous solution to 6.0-7.0, filtering to obtain potassium fluorosilicate; continuing to adjust the pH of the filtered metal cation concentrated aqueous solution to alkaline, filtering to obtain aluminum hydroxide and aluminum precipitation mother liquor;
[0052] S10. Evaporation crystallization, freezing crystallization: The aluminum precipitation mother liquor is subjected to an evaporation crystallization process, and after evaporation to sodium salt saturation, potassium salt and evaporation mother liquor are separated by filtration, and sodium salt and potassium salt are separated by a step-by-step freezing crystallization process on the evaporated mother liquor. The production method of sodium salt and potassium salt is not limited thereto, and the present invention does not limit the process of producing sodium salt and potassium salt;
[0053] S11. Distilled water washing: collecting distilled water produced in each evaporation process section, using it to dilute the leaching solution in step S1, and washing the leaching residue in step S1 (or using it to prepare a saturated solution for each product to wash each product), and the leaching residue obtained after washing is used as a raw material for producing building materials, and generating acidic washing water;
[0054] S12. Acid concentration: The nanofiltration acid-purified freshwater liquid in S2, the high-pressure nanofiltration freshwater in S4, the electrodialysis acid liquid, and the acid wash water in S11 are subjected to acid concentration treatment separately or collectively to obtain concentrated acid which is reused as leaching acid in the leaching step S1.
[0055] Step S1 Leaching step The process method is to use fluorosilicic acid mixed with other inorganic acids as leaching acid to destroy the lithium mica structure to achieve leaching, avoid the high energy consumption problem caused by high-temperature roasting and leaching, reduce the equipment material requirements and increase the leaching rate of each valuable metal. Most of the valuable metals will be converted into soluble salts and enter the leachate. The main components of the remaining leaching residue are silicon dioxide and a small amount of aluminum silicate (or fluorosilicate, silicon phosphate), which can be used as raw materials for manufacturing building materials after washing to remove residual acid.
[0056] There are charged groups on the surface of nanofiltration membrane or in the membrane, which, through electrostatic interaction, hinder the penetration of multivalent ions. Based on this characteristic, nanofiltration membrane can be used to separate hydrogen ions and metal ions in solution, or to separate high and low valent metal ions, to achieve the purpose of acid purification and separation of metal ions. In order to separate various types of valuable metals in the leachate and avoid the generation of fluorine-containing wastewater, step S2 uses an acid-resistant nanofiltration membrane to perform membrane separation on the leachate, recovers most of the leaching acid and fluorine element, makes the pH adjustment, precipitation and impurity removal alkali consumption greatly reduced, and avoids the problem of high energy consumption of thermal defluorination treatment at the same time, the material requirements of the reaction equipment are reduced, and there is no need to increase the fluorine-containing waste gas collection equipment. Step S3 uses an acid-resistant nanofiltration membrane to separate metal cation fresh water liquid and high-valent metal cation (mainly aluminum) concentrated water liquid.
[0057] The main metal elements in the metal cation freshwater solution are potassium, lithium, sodium, rubidium, and cesium. Step S4 uses a high-pressure nanofiltration membrane for further concentration and then uses a bipolar membrane electrodialysis process to produce an acid solution containing a mixed acid and a mixed alkali solution. The bipolar membrane electrodialysis process achieves the three goals of product defluorination purification, lithium salt solution causticization, and acid recycling in one step, greatly reducing the amount of defluorinating agents and acid-base auxiliary materials. The causticized lithium solution is conducive to crystallization separation and carbonization separation of lithium elements; the causticized lithium precipitation mother liquor greatly reduces the alkali consumption for adjusting pH and saponification before extraction, making each product higher in purity; the causticized raffinate is used for step S9 defluorination and aluminum precipitation to adjust pH, reducing the alkali consumption.
[0058] Step S5 utilizes the low solubility of lithium hydroxide monohydrate to concentrate the mixed alkali solution with an alkali-resistant reverse osmosis membrane, evaporation concentration, and cooling crystallization process to obtain lithium hydroxide monohydrate crystals, which are then washed and dried to prepare a battery-grade lithium hydroxide monohydrate product. The crystallization mother liquor is returned to the evaporation concentration process section and circulated until the potassium hydroxide is saturated to obtain a saturated crystallization mother liquor.
[0059] Step S6: carbon dioxide is introduced into the saturated crystallization mother liquor to carbonize the precipitated lithium and further improve the utilization rate of the leached lithium, thereby obtaining lithium carbonate and the precipitated lithium mother liquor. The lithium carbonate can be washed and dried to prepare battery-grade lithium carbonate.
[0060] The main components of the lithium precipitation mother liquor are strong alkalis such as potassium, sodium, rubidium and cesium, which are beneficial to improving the extraction efficiency and separation efficiency under high alkalinity conditions. Step S7 separates high-value rubidium salt stripping solution and cesium salt stripping solution through multi-stage extraction and stripping.
[0061] The alkaline raffinate is used to adjust the pH of the metal cation concentrated aqueous solution in step S9 after oil removal, and the fluorine element in the solution is removed by generating insoluble potassium fluorosilicate, thereby avoiding the use of additional defluorinating agents, producing aluminum hydroxide and aluminum precipitation mother liquor, reducing the alkali consumption for callback, and reducing production costs.
[0062] Step S10 evaporates the aluminum precipitation mother liquor to produce potassium salt and sodium salt. After the aluminum precipitation mother liquor is subjected to heavy metal adsorption resin to remove trace heavy metals therein, potassium salt is produced and can be sold as potash fertilizer.
[0063] The mixed acid-containing wastewater generated by each nanofiltration process section, bipolar membrane process section, and residual acid washing process section can be recycled into the leaching process section by producing concentrated acid through the acid concentration process in step S12, thereby recycling the fluorine element and avoiding the treatment and emission problems of fluorine-containing wastewater and waste gas.
[0064] The beneficial effects of the present invention are:
[0065] (1) The method of the present invention has mild leaching reaction conditions, low energy consumption, high leaching rate of valuable metals, and most of the fluorine-containing leaching acid is collected and reused. No additional equipment is required for pyrolysis of the leaching solution and collection and treatment of the fluorine-containing waste gas, and the alkali consumption for pH adjustment precipitation and impurity removal is greatly reduced.
[0066] (2) The bipolar membrane electrodialysis process in the method of the present invention achieves the three purposes of defluorination purification of the product liquid, causticization of the lithium salt solution, and separation acid recycling in one step, greatly reducing the amount of various auxiliary materials used and reducing the production cost of lithium mica.
[0067] (3) In the method of the present invention, each valuable metal in the lithium mica is extracted as much as possible to prepare a qualified product, and the metal loss of each mother liquor and waste liquid is extremely small, and the unit lithium mica production income is improved.
[0068] (4) In the method of the present invention, the products of each process are effectively disposed of, and no fluorine-containing wastewater or waste gas is discharged to external treatment. All polluting elements are fixed in solid substances, which generate economic value as products. It is green, environmentally friendly, and friendly to the natural environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 This is a schematic diagram of the process of Example 1 of the present invention;
[0070] Figure 2 This is the XRD diagram of the solid waste obtained in Example 1 of the present invention;
[0071] Figure 3This is the XRD diagram of the solid waste obtained in Example 6 of the present invention. DETAILED DESCRIPTION
[0072] The present invention will be further described below in conjunction with specific embodiments.
[0073] The main components of the lithium mica raw material used in the embodiment of the present invention are shown in Table 1:
[0074] Table 1. Main components of lepidolite
[0075]
[0076] Embodiment 1:
[0077] A method for comprehensive utilization of lepidolite, such as Figure 1 As shown, the following steps are included:
[0078] S1. Low temperature leaching: Add a leaching acid having a hydrogen ion concentration of 8 mol / L to a 100 mesh lithium mica ore powder, wherein the leaching acid is prepared by mixing 30% by mass fluorosilicic acid and 50% by mass concentrated sulfuric acid with an amount of 5 times the mass of the lithium mica ore powder, react at 95°C, 0.2MPa for 3h, cool to room temperature after the reaction, add distilled water to dilute to a hydrogen ion concentration of 5mol / L, and filter and separate to obtain a leachate and a leach residue;
[0079] S2. Nanofiltration acid purification: The leachate is subjected to acid purification using a 5-grade AR40-35 nanofiltration membrane, and the pressure before the nanofiltration membrane is maintained at 1.5 MPa to obtain nanofiltration acid-purified concentrated water and nanofiltration acid-purified fresh water;
[0080] S3. Nanofiltration cation separation: The nanofiltration acid purified concentrated water solution is treated with a 3-stage AR50-35 nanofiltration membrane for cation separation. The pressure before the nanofiltration membrane is maintained at 2.5 MPa to obtain a monovalent metal cation fresh water solution and a high-valent metal cation concentrated water solution;
[0081] S4. High-pressure nanofiltration concentration and bipolar membrane electrodialysis: The monovalent metal cation freshwater is concentrated by a 7-level AR10-35 high-pressure nanofiltration membrane to obtain high-pressure nanofiltration freshwater and high-pressure nanofiltration concentrated water. The high-pressure nanofiltration concentrated water is subjected to bipolar membrane electrodialysis. The electrodialysis device used contains a raw liquid chamber, an electrodialysis alkali liquid chamber and an electrodialysis acid liquid chamber. The electrodialysis alkali liquid chamber and the raw liquid chamber are separated by a cation membrane, and the electrodialysis acid liquid chamber and the raw liquid chamber are separated by an anion membrane. The cation membrane and the anion membrane are arranged alternately, and each pair of anion and cation membranes are separated by a bipolar membrane. The electrodes of the bipolar membrane electrodialysis device are titanium-plated ruthenium-iridium electrodes, and the electrode liquid is a lithium hydroxide solution with a mass percentage concentration of 2% and a current density of 250A / m 2 After 3h electrodialysis, the alkali liquid chamber OH -The molar concentration reaches 2.2 mol / L, and electrodialysis acid solution and electrodialysis alkali solution are obtained;
[0082] S5. Evaporation concentration and cooling crystallization: The electrodialysis alkali solution is treated by evaporation concentration process, the solution volume is reduced by 60%, and after the potassium hydroxide component is saturated at room temperature, the evaporated concentrated solution is cooled to 20°C, and filtered to obtain lithium hydroxide monohydrate crystals and crystal mother liquor. The lithium hydroxide monohydrate crystals are washed twice with saturated lithium hydroxide solution, and dried at 90°C to obtain battery-grade lithium hydroxide monohydrate with a main lithium hydroxide content of 56.9%;
[0083] S6. Carbonization of precipitated lithium: carbon dioxide is introduced into the crystallization mother liquor until the lithium content in the filtrate is less than 100 mg / L, and lithium carbonate and precipitated lithium mother liquor are obtained after filtration. The lithium carbonate is washed with nitrilotriacetic acid (NTA) solution and dried at 120°C to obtain a battery-grade lithium carbonate product with a purity of 99.5%;
[0084] S7. Multi-stage extraction separation and stripping: t-BAMBP and sulfonated kerosene are combined in a mass ratio of 35:65 to form an extraction organic phase. The lithium precipitation mother liquor is subjected to 6-stage countercurrent extraction at an extraction ratio (oil-water ratio) of 1.2:1 at 25°C to obtain a preliminary loaded organic phase and a raffinate. The preliminary loaded organic phase is subjected to a 3-stage water washing process at a water washing ratio (oil-water ratio) of 1:1 to obtain a washed loaded organic phase and wash water. The wash water is mixed into the raffinate. The washed loaded organic phase is subjected to a 2-stage stripping treatment at a stripping ratio (oil-water ratio) of 2:1. The 1st and 2nd stage stripping acids are 2mol / L and 4mol / L hydrochloric acid, respectively. Stripping solution A is obtained by the first stripping, and stripping solution B is obtained by the second stripping. The raffinate, stripping solution A, and stripping solution B are pre-treated with activated carbon for oil removal until the oil content is less than 5mg / L;
[0085] S8. Evaporation and crystallization: The stripping solutions A and B are evaporated and crystallized respectively to produce corresponding rubidium chloride and cesium chloride products with purities of 99.4% and 99.1%, respectively;
[0086] S9. Fluorine removal and aluminum precipitation: Use the raffinate after oil removal and KOH to adjust the pH of the high-valent metal cation concentrated aqueous solution to 6.5, produce potassium fluorosilicate precipitation, filter and remove the precipitate to obtain the defluorine filtrate, and the fluorine in the defluorine filtrate is reduced to 76 mg / L. Use sodium hydroxide to adjust the pH of the defluorine filtrate to 9, filter to obtain aluminum hydroxide and aluminum precipitation mother liquor;
[0087] S10. Evaporation crystallization, frozen crystallization: The aluminum precipitation mother liquor is evaporated and crystallized until the solution volume is reduced by 84%, and potassium sulfate is obtained by filtration. The mass fraction of K2O in potassium sulfate is 51%. The mother liquor is frozen and evaporated to 0°C and filtered to obtain sodium sulfate decahydrate crystals. The sodium sulfate dehydrate can be obtained by heating and dehydrating at 100°C for sale;
[0088] S11. Distilled water washing: distilled water produced in each evaporation process section is collected and used to dilute the leaching solution in step S1, or to wash the leaching residue in step S1, to obtain solid waste and acidic washing water. The XRD pattern of the obtained solid waste is as follows: Figure 2 As shown, the crystals are mainly SiO2 and Na2SiF6 as determined by XRD, and the solid waste is used as raw material for producing building materials;
[0089] S12. Acid concentration: Perform falling film evaporation on the nanofiltration acid-purified fresh water, high-pressure nanofiltration fresh water, electrodialysis acid solution and acid wash water to obtain a mixed acid solution with a mass percentage concentration of 33% as leaching acid for reuse in step S1.
[0090] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 92%, 91%, 97%, 96% and 79% respectively.
[0091] Embodiment 2:
[0092] A method for comprehensive utilization of lepidolite is carried out according to the steps in Example 1, except that:
[0093] In step S2, the number of nanofiltration membrane stages is 7;
[0094] In step S3, the number of nanofiltration membrane stages is 5;
[0095] In step S7, the oil removal process is a combined ozone oxidation and activated carbon oil removal process, and the raffinate, stripping solution A, and stripping solution B are pre-treated for oil removal until the oil content is less than 1 mg / L;
[0096] The purity of the rubidium chloride and cesium chloride products obtained in step S8 is increased to 99.8% and 99.5%.
[0097] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 93%, 90%, 97%, 97% and 82% respectively.
[0098] Embodiment 3:
[0099] A method for comprehensive utilization of lepidolite is carried out according to the steps in Example 1, except that:
[0100] In step S1, the low-temperature leaching reaction conditions are 140°C, 0.4MPa, and the reaction time is 1.5h;
[0101] In step S7, the oil removal process is a combined ozone oxidation and activated carbon oil removal process, and the raffinate, stripping solution A, and stripping solution B are pre-treated for oil removal until the oil content is less than 1 mg / L;
[0102] The purity of the rubidium chloride and cesium chloride products obtained in step S8 is increased to 99.7% and 99.5%;
[0103] In step S9, the pH of the high-valent metal cation concentrated aqueous solution is adjusted to 7 using the deoiled raffinate to produce potassium fluorosilicate precipitate, which is filtered to remove the precipitate, and the fluorine content of the solution is reduced to 72 mg / L;
[0104] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 95%, 91%, 97%, 97% and 84% respectively.
[0105] Embodiment 4:
[0106] A method for comprehensive utilization of lepidolite is carried out according to the steps in Example 1, except that:
[0107] In step S2, the number of nanofiltration membrane stages is 3;
[0108] In step S5, the electrodialysis alkali solution is concentrated by using an alkali-resistant reverse osmosis membrane to a Li content of 34.7 g / L, and then evaporated and concentrated until the volume of the solution is reduced by 67%. The concentrated solution is cooled to 0° C. and filtered to obtain lithium hydroxide monohydrate crystals.
[0109] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 88%, 93%, 96%, 95% and 80% respectively.
[0110] Embodiment 5:
[0111] A method for comprehensive utilization of lepidolite is carried out according to the steps in Example 1, except that:
[0112] In step S1, the concentration of leaching acid hydrogen ions is 6 mol / L, the leaching acid is prepared by mixing 30% fluorosilicic acid and 37.5% hydrochloric acid, the amount of leaching acid is 3.5 times the mass of the lithium mica ore powder, and the leaching reaction conditions are 100° C., 0.3 MPa, and the reaction time is 2 hours;
[0113] In step S10, the aluminum precipitation mother liquor is evaporated and crystallized until the volume of the solution is reduced by 62%, and the salt produced is potassium chloride. The salt produced by cooling is potassium chloride, and the remaining mother liquor is a mixed solution of potassium chloride and sodium chloride;
[0114] In step S12, the mixed acid is subjected to falling film evaporation to obtain a mixed acid solution with a mass percent concentration of 29%.
[0115] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 93%, 85%, 97%, 96% and 82% respectively.
[0116] Embodiment 6:
[0117] A method for comprehensive utilization of lepidolite is carried out according to the steps in Example 1, except that:
[0118] In step S1, the concentration of leaching acid hydrogen ions is 8 mol / L, the leaching acid is prepared by mixing 30% fluorosilicic acid and 85% phosphoric acid, the mass of the leaching acid is twice the mass of the lithium mica ore powder, and the leaching reaction conditions are 80° C., 0.2 MPa, and the reaction time is 4 hours;
[0119] In step S9, after adjusting the pH to 6.5, the precipitate is a mixture of aluminum phosphate and potassium fluorosilicate. After adjusting the pH to 9, only a small amount of aluminum hydroxide containing aluminum phosphate is produced;
[0120] In step S10, the aluminum precipitation mother liquor is evaporated to produce potassium salt, which is potassium phosphate, and can be used as phosphorus and potassium fertilizer. The sodium salt produced by cooling and crystallization is sodium phosphate dodecahydrate;
[0121] The XRD pattern of the solid waste after washing in step S11 is as follows: Figure 3 As shown, XRD detection shows that the main components of its crystal are silicon dioxide and silicon phosphate;
[0122] In step S12, falling film evaporation is used to concentrate the mixed acid to a mass percentage concentration of 32%.
[0123] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 90%, 93%, 95%, 93% and 45% respectively.
[0124] Comparative Example 1:
[0125] A method for comprehensive utilization of lepidolite comprises the following steps:
[0126] S1. High temperature calcination for defluorination, leaching: adding 10% of water by mass to the lithium mica powder of Example 1, and then calcining at 800 ° C for 1h, the calcined product was ball-milled to 100 mesh, 50% of water was added to the calcined product for slurrying, 120% of the theoretical amount of nitric acid was added to the slurry, and the reaction was carried out at 100 ° C for 1h, and then filtered to obtain leached residue and leachate;
[0127] S2. Leaching residue washing: The leaching residue obtained in S1 is washed and treated as building materials or solid waste;
[0128] S3. Nanofiltration separation: The leachate obtained in S1 is treated with a 3-stage AR50-35 nanofiltration membrane for cation separation. The pressure before the nanofiltration membrane is maintained at 2.5 MPa. After separation by the nanofiltration membrane, a monovalent ion nitrate solution and a multivalent ion nitrate solution are obtained;
[0129] S4. Separation and purification of monovalent ion nitrate solution: t-BAMBP and sulfonated kerosene are used in a mass ratio of 35:65 to form an organic phase for extraction. The monovalent ion nitrate solution obtained in S3 is subjected to 6-stage countercurrent extraction at an extraction phase ratio (oil-water ratio) of 1.2:1 at 25°C to obtain a loaded organic phase and a raffinate. The loaded organic phase is subjected to a 2-stage stripping treatment at a stripping phase ratio (oil-water ratio) of 2:1, and the stripping acid is 4 mol / L hydrochloric acid to obtain a stripping solution. After the stripping solution is neutralized with potassium hydroxide, the neutralized stripping solution is further purified by a two-stage selective ion exchange resin process to obtain a potassium adsorption solution, a primary resin desorption solution containing rubidium, and a resin desorption solution containing cesium, respectively. The raffinate is a lithium nitrate solution.
[0130] S5. Impurity removal of polyvalent ion nitrate solution: Heat the polyvalent ion nitrate solution in S3 to 40°C, add magnesium oxide or calcium oxide to adjust the pH to 7, and produce a precipitate of aluminum hydroxide, which can be used in aluminum plants. The remaining liquid is evaporated and concentrated to obtain a calcium magnesium nitrate solution, add calcium oxide or magnesium oxide, etc., adjust the concentration and proportion of the system, and then concentrate and spray granulate to produce calcium magnesium nitrate fertilizer.
[0131] S6. Bipolar membrane separation: The lithium nitrate solution obtained in S4 is concentrated, enriched, and finely filtered, and then separated by a bipolar membrane to obtain dilute nitric acid and lithium hydroxide solution. The dilute nitric acid is concentrated and recycled back to the leaching process, and the lithium hydroxide solution is evaporated, concentrated, and crystallized to produce high-purity lithium hydroxide products.
[0132] The recovery rates of lithium, potassium, rubidium, cesium and aluminum in a single cycle process are 80%, 86%, 81%, 82% and 87% respectively.
[0133] In Comparative Example 1, a large amount of alkali is consumed in the direct extraction and separation of the monovalent ion nitrate solution, and the residual acid is not effectively recovered. The cost of using magnesium oxide to remove impurities in the multivalent ion solution is relatively high, and the overall acid recovery rate of the process is low and the cost of adding drugs is high. In the embodiment, most of the residual acid is recovered by multi-stage nanofiltration separation. In the embodiment, the operating cost of the extraction system is reduced by removing impurities through a bipolar membrane, producing lithium carbonate, and then extracting and separating two high-value metals, rubidium and cesium, from the lithium precipitate mother liquor. The sodium and potassium raffinate is directly used as a pH regulator, which reduces the amount of alkali consumed for impurity removal.
[0134] Combining the above embodiments and comparative examples, it can be seen that this method not only improves the recovery rate of valuable metals, but also eliminates the calcination cost and greatly reduces the cost of adding drugs, and has no waste gas output, showing significant advantages in overall production cost and environmental friendliness.
Claims
1. A method for comprehensive utilization of lepidolite, Features: The following steps are involved: (1) mixing lepidolite ore powder with leaching acid, leaching, and filtering to obtain a leachate and a leaching residue; (2) subjecting the leaching solution obtained in step (1) to nanofiltration acid purification, nanofiltration cation separation and high-pressure nanofiltration concentration in sequence to obtain high-pressure nanofiltration fresh water and high-pressure nanofiltration concentrated water, and subjecting the high-pressure nanofiltration concentrated water to electrodialysis to obtain electrodialysis acid solution and electrodialysis alkali solution; (3) evaporating and concentrating the electrodialysis alkali solution obtained in step (2) and then cooling and crystallizing it, filtering to obtain lithium hydroxide monohydrate crystals and a crystallization mother liquor, introducing carbon dioxide into the crystallization mother liquor, and filtering to obtain lithium carbonate and lithium precipitation mother liquor after the reaction; (4) extracting the lithium precipitated mother liquor obtained in step (3) to separate a loaded organic phase and a raffinate, stripping the loaded organic phase with a stripping acid to obtain a stripping solution A and a preliminary stripping organic phase, further stripping the preliminary stripping organic phase with a stripping acid to obtain a stripping solution B, evaporating and crystallizing the stripping solution A to produce a rubidium salt, and evaporating and crystallizing the stripping solution B to produce a cesium salt; (5) The pH of the metal cation concentrated aqueous solution produced by the nanofiltration cation separation is adjusted to 6.0-7.0, and potassium fluorosilicate and a filtrate are obtained by filtering. The pH of the filtrate is further adjusted to alkaline, and aluminum hydroxide and aluminum precipitation mother liquor are obtained by filtering.
2. A method for comprehensive utilization of lepidolite according to claim 1, Features: The following steps are also included: After the aluminum precipitation mother liquor obtained in step (5) is evaporated to saturation with sodium salt, the sodium salt and potassium salt are separated by a step-by-step freezing crystallization process.
3. A method for comprehensive utilization of lepidolite according to claim 2, Features: The following steps are also included: The distilled water produced by evaporation and concentration of the electrodialysis alkali solution, evaporation and crystallization of the stripping solution A, evaporation and crystallization of the stripping solution B, and evaporation of the aluminum precipitation mother solution is collected and used to dilute the leaching solution in step (1).
4. A method for comprehensive utilization of lepidolite according to claim 1, Features: The following steps are also included: At least one of the nanofiltration acid-purified fresh water produced by the nanofiltration acid purification, the high-pressure nanofiltration fresh water, the electrodialysis acid solution and the acidic washing water obtained after washing the leaching residue is subjected to acid concentration for preparing the leaching acid in step (1).
5. A method for comprehensive utilization of lepidolite according to claim 1, Features: In step (1), the leaching acid is a mixture of fluorosilicic acid and other inorganic acids, and the other inorganic acids include at least one of hydrochloric acid, sulfuric acid and phosphoric acid.
6. A method for comprehensive utilization of lepidolite according to claim 1, Features: In step (1), the leaching temperature is 80-150° C., the leaching pressure is 0.1-1.0 MPa, and the leaching reaction time is 1-4 hours.
7. A method for comprehensive utilization of lepidolite according to claim 1, Features: In step (2), the nanofiltration acid purification is to perform acid purification on the leachate through a nanofiltration membrane to obtain a nanofiltration acid-purified concentrated water solution and a nanofiltration acid-purified fresh water solution, and the nanofiltration acid-purified concentrated water solution enters the nanofiltration cation separation step.
8. A method for comprehensive utilization of lepidolite according to claim 7, Features: In step (2), the nanofiltration cation separation is to perform cation separation treatment on the nanofiltration acid purified concentrated water solution through a nanofiltration membrane to obtain a metal cation fresh water solution and the metal cation concentrated water solution, and the metal cation fresh water solution enters the high-pressure nanofiltration concentration step.
9. A method for comprehensive utilization of lepidolite according to claim 1, Features: In step (4), the stripping solution A and the stripping solution B are both subjected to oil removal pretreatment before evaporation and crystallization so that the oil in the stripping solution A and the stripping solution B is reduced to below 5 mg / L.
10. A method for comprehensive utilization of lepidolite according to claim 1, Features: In step (5), the adjusting agent used to adjust the pH is at least one of KOH, NaOH and the raffinate, and adjusting the pH of the filtrate to alkaline means adjusting the pH to 8.0-9.0.
Citation Information
Patent Citations
Comprehensive utilization method for directly extracting lithium by silicate-based lithium-containing ore acid process
CN110526250A
Method for preparing battery-grade lithium hydroxide from lepidolite
CN111268701A
Preparation method of lithium hydroxide
CN111924861A
Method for comprehensively recovering lithium, rubidium and cesium from lithium ore leachate
CN116623009A
Lithium hydroxide preparation method
WO2020207223A1
Cited By
Soda ash and sodium bicarbonate production method