Method for enriching platinum, palladium and rhodium from automobile ternary waste catalyst by wet process
By carrying out the Fenton oxidation activation and oxidative leaching steps in the same reactor, the problems of high investment in pyrometallurgical enrichment equipment and low recovery rate in hydrometallurgical enrichment are solved, realizing a highly efficient precious metal recovery and an environmentally friendly platinum, palladium, and rhodium recovery process.
Patent Information
- Application Number
- CN202410923687.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing pyrometallurgical enrichment processes involve large investments, high energy consumption, and complicated post-enrichment processing of the enriched gold. Hydrometallurgical enrichment processes have low precious metal recovery rates, especially for rhodium, where the leaching rate is difficult to exceed 80%.
The process employs a combination of Fenton oxidation activation and oxidative leaching steps, carried out in the same reactor. Through the combination of FeCl2, MgCl2, and hydrochloric acid, platinum, palladium, and rhodium are oxidized into chloride complexes by FeOOH active ions and chloride ions provided by magnesium chloride under strong oxidizing conditions. The precious metals are then replaced by iron powder, and the replacement wastewater is finally recycled.
It improves the wet leaching rate and recovery rate of precious metals, shortens the process flow, reduces wastewater discharge, lowers equipment investment and energy consumption, and simplifies subsequent treatment.
Smart Images

Figure CN118996137A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recovering precious metals from automobile waste catalysts, and in particular to a method for wet-process enrichment of platinum, palladium and rhodium from automobile ternary waste catalysts. Background Art
[0002] Automobile three-way catalysts generally use platinum group metals such as platinum, palladium and rhodium as active components. With the rapid development of my country's automobile industry, the number of cars in use has increased rapidly year by year. At the same time, my country has gradually entered the peak period of car scrapping, and a large number of scrapped automobile three-way catalysts urgently need to be processed and developed and utilized.
[0003] The content of platinum group metals in spent automobile catalysts reaches more than 0.1%, which is hundreds or even thousands of times higher than the grade of ordinary ore. 6% to 8% of my country's platinum, 75% of palladium and almost all rhodium are used in the manufacture of automobile exhaust purification catalysts. The growth of automobile consumption has led to an increasing demand for platinum group metals. However, my country's platinum group metal resources are scarce, the contradiction between supply and demand is prominent, and it is highly dependent on imports. The explosive growth of waste automobile three-way catalysts has become a mobile mine of platinum group metals, which has great development value.
[0004] The recovery of platinum group metals from scrap automobile three-way catalysts is mainly divided into three stages: enrichment, separation and refining. The primary core step of the whole process is efficient enrichment, which mainly includes two processes: pyrometallurgical and hydrometallurgical.
[0005] At present, most recycling companies at home and abroad mainly use pyrometallurgical enrichment technology, which is a process of enriching platinum group metals at a high temperature of 1400-1600℃ using base metals such as iron and copper as collectors. Its advantages are high recovery rate of platinum group metals and large enrichment ratio, but it has disadvantages such as special equipment, large equipment investment, high energy consumption, and troublesome subsequent treatment of enriched alloys.
[0006] Wet enrichment is to wet-leach the precious metals in the catalyst at room temperature and pressure, and then selectively precipitate and enrich to obtain precious metal-enriched slag. The wet enrichment process and equipment are simple, with low energy consumption, low production cost, and simple subsequent refining process. However, the existing wet process has the problem of low precious metal leaching rate, especially the leaching rate of rhodium is difficult to exceed 80%, and the precious metal recovery rate is low. Summary of the invention
[0007] The purpose of the present invention is to design a method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, so as to solve the shortcomings of the pyrometallurgical enrichment process mentioned in the background technology, such as large equipment investment, high energy consumption, and troublesome subsequent treatment of the enriched alloy, as well as the problem of low recovery rate of precious metals in the wet enrichment process.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0010] a. Crushing: crushing the ternary waste catalyst into powder;
[0011] b. Fenton oxidation activation: Add the material and auxiliary materials into the reactor in a mass ratio of material: water: MgCl2: FeCl2 = 1:4:1-2:0.2-1, stir and mix, heat to 50-90°C and maintain, slowly drop hydrogen peroxide and 36% mass fraction hydrochloric acid, and activate leaching for 1-3h;
[0012] FeCl2 provides Fe 2+ Under weak acidic conditions, it reacts with hydrogen peroxide to produce FeOOH active ions. The oxidation potential of FeOOH active ions under weak acidic conditions can reach 2.73V, which has strong oxidizing properties. The magnesium chloride and ferric chloride in the solution provide sufficient chloride ion concentration. Under high chloride ion concentration and strong oxidizing conditions, platinum, palladium and rhodium are oxidized into chloride complex ions and dissolved in the solution. The reaction is:
[0013]
[0014] During the Fenton reaction, the Fenton reaction increases the strong oxidizing property and promotes the leaching of platinum, palladium and rhodium. 3+ Hydrolysis into active iron hydroxide colloid will adsorb part of the platinum, palladium and rhodium dissolved in the solution into the iron hydroxide colloid precipitation, thereby reducing the content of the noble metals dissolved in the solution and promoting the oxidation and dissolution of the noble metals in the solution. The dissolved noble metals are adsorbed and precipitated by the iron hydroxide colloid, thus playing the role of activating the noble metals.
[0015] c. Oxidative leaching: After the activation leaching is completed, add 36% mass fraction hydrochloric acid to the reactor, slowly add saturated sodium chlorate solution at 70-80°C, and oxidatively leach for 1-2 hours;
[0016] After the activation leaching is completed, hydrochloric acid is added to dissolve the iron hydroxide precipitate and release the active components of the precious metals. Then, a saturated sodium chlorate solution is added to oxidize and dissolve the precious metals. The decomposition of sodium chlorate and hydrochloric acid has strong oxidizing properties, thereby increasing the dissolution rate of the precious metals.
[0017] d. Filtration 1: After the oxidation leaching is completed, the filtrate L1 and the filter residue S1 are obtained by filtration and washing. The filter residue S1 is a mixture of alumina and silicon oxide, which is a catalyst carrier, and can be sold;
[0018] e. Replacement enrichment: The filtrate L1 is added to a stirring tank, and then iron powder or iron block is added to stir and replace the precious metals, namely platinum, palladium and rhodium. The replacement time is 1-8h. After the replacement, the solution is sampled to detect the residual amount of precious metals and proceed to the next step;
[0019] Add iron powder or iron block to replace and enrich precious metals. The reaction principle is as follows:
[0020] Fe+Fe 3+ =Fe 2+ ;
[0021]
[0022] f. Filtration 2: After the replacement is completed, filter and wash to obtain the filtrate L2 and the filter residue S2.
[0023] The main components of the filtrate L2 obtained by filtration after iron replacement are still FeCl2+MgCl2. After adding a small amount of magnesium oxide to the filtrate L2 to adjust the pH, it can return to step b to oxidize and activate the precious metals.
[0024] Furthermore, in the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, in step a, the ternary waste catalyst is crushed into 40-100 mesh powder to expose the precious metals on the surface of the material so as to activate and leach the precious metals.
[0025] Furthermore, in the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, the volume of hydrogen peroxide added dropwise per hour in step b is 0.5-2 times the mass value of FeCl2. If it is too fast, the decomposition rate of hydrogen peroxide will be fast, resulting in high reagent consumption, and if it is too slow, the Fenton oxidation activation will be insufficient.
[0026] Furthermore, in the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, hydrochloric acid is slowly added dropwise in step b to maintain the pH of the entire reaction system at 1.5-4. If the pH is too low, the Fenton reaction effect will be affected, and if it is too high, divalent iron will be precipitated.
[0027] Furthermore, in the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, the volume of hydrochloric acid in step c is 0.5-2 times the mass value of the material.
[0028] Furthermore, in the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, the volume of the saturated sodium chlorate solution in step c is 0.1-1 times the mass value of the material.
[0029] Furthermore, in the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, the amount of iron powder or iron block added in step e is excessive so as to fully replace the precious metals.
[0030] Furthermore, the above-mentioned method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst also includes step g for replacing tail liquid for reuse: adding magnesium oxide to the filtrate L2, adjusting the pH to be greater than 1 and returning to step b for recycling.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The present invention improves the activity of precious metals by setting up Fenton oxidation activation, thereby improving the wet leaching rate and recovery rate of precious metals;
[0033] 2. The Fenton oxidation process and the oxidation leaching process of the present invention are completed in the same reactor, thus shortening the process flow;
[0034] 3. The amount of enriched slag after iron replacement is small and the enrichment multiple is high, which is convenient for the subsequent separation and purification of platinum, palladium and rhodium, and there is no problem of difficult treatment of ferrosilicon alloys from pyrometallurgical enrichment;
[0035] 4. The replacement wastewater of this process can be recycled to the Fenton oxidation activation step, which can reduce the wastewater discharge in the process and is green and environmentally friendly;
[0036] 5. The equipment used in the present invention is simple, the investment is small, and the energy consumption is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0038] The present invention can be implemented in a variety of variations and in various ways, but as an example, a specific implementation is described in detail below. The implementation is not limited to the specific way of the present invention disclosed herein, and all variations, equivalents, and alternatives implemented within the scope explicitly stated in the attached claims are included in the object. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] Take 6 kg of the three-way catalyst, grind it to 80 mesh with a disc mill, take samples for analysis, and the main components of the three-way catalyst are shown in Table 1 below:
[0040] Table 1:
[0041] Ingredients <![CDATA[Al2O3]]> <![CDATA[SiO2]]> MgO <![CDATA[ZrO2]]> CeO Pt Pd R other Content (g / t) 373000 334000 91000 48000 38000 236 1642 203 114000
[0042] The three-way spent catalysts used below all come from this three-way catalyst.
[0043] Example 1
[0044] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0045] a. Crushing: Using the above-mentioned crushed 80 mesh three-way catalyst powder;
[0046] b. Fenton oxidation activation: put 1kg of material powder into a 10L reactor, add 4L of water, 1kg of MgCl2 and 200g of FeCl2, stir and mix, heat to 60°C and maintain the temperature, slowly add hydrogen peroxide and 36% mass fraction hydrochloric acid, the hydrogen peroxide drop acceleration rate is 150mL / h, the hydrochloric acid drop acceleration rate is to keep the solution reaction pH = 2-3, and stop adding hydrogen peroxide and hydrochloric acid after 1.5h of activation leaching;
[0047] c. Oxidative leaching: After the activation leaching is completed, add 500mL of 36% mass fraction hydrochloric acid to the reactor, heat to 80°C, slowly add 200mL of saturated sodium chlorate solution, and oxidatively leach for 1h;
[0048] d. Filtration 1: After the oxidation leaching is completed, the filtrate is filtered and washed to obtain a filtrate L1 and a filter residue S1. By analyzing and detecting the filtrate L1 and the filter residue S1, the leaching rates of platinum, palladium and rhodium precious metals are: platinum 99.1%, palladium 99.4%, and rhodium 95.3%;
[0049] e. Replacement enrichment: The filtrate L1 was added to a stirring tank, and then 80g of iron powder was added and stirred to replace the precious metals. The replacement time was 6h. After the replacement, the solution was sampled and tested. The contents of platinum, palladium and rhodium in the solution were measured as follows: platinum 5.6ppm, palladium 3.8ppm, rhodium 8ppm, and the next step was performed.
[0050] f. Filtration 2: After the replacement is completed, the filtrate is filtered and washed to obtain the filtrate L2 and the filter residue S2. The filter residue S2 is dried and weighed to be 23.3g. The contents of platinum, palladium and rhodium are: platinum 0.99%, palladium 7.01%, rhodium 0.827%, and the enrichment multiple of precious metals is 43 times.
[0051] Example 2 (Reuse of replacement tail liquid)
[0052] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0053] a. Crushing: Using the above-mentioned crushed 80 mesh three-way catalyst powder;
[0054] b. Fenton oxidation activation: 1 kg of material powder was put into a 10 L reactor, 5 L of the filtrate L2 in Example 1 was added, magnesium oxide was slowly added to adjust the pH to 3 after stirring, heated to 70 ° C and maintained at this temperature, hydrogen peroxide and 36% mass fraction hydrochloric acid were slowly added dropwise, the hydrogen peroxide drop rate was 100 mL / h, and the hydrochloric acid drop rate was to keep the solution reaction pH = 2.5-3, and the hydrogen peroxide and hydrochloric acid were stopped after 2 hours of activation leaching;
[0055] c. Oxidative leaching: After the activation leaching is completed, add 500mL of 36% mass fraction hydrochloric acid to the reactor, heat to 85°C, slowly add 300mL of saturated sodium chlorate solution, and oxidatively leach for 1h;
[0056] d. Filtration 1: After the oxidation leaching is completed, the filtrate L1 and the filter residue S1 are obtained by filtering and washing. The leaching rates of platinum, palladium and rhodium precious metals in the filtrate L1 and the filter residue S1 are analyzed and detected: platinum 99.2%, palladium 99.5%, and rhodium 94.8%;
[0057] e. Replacement enrichment: The filtrate L1 was added to a stirring tank, and then 100g of iron powder was added and stirred to replace the precious metals. The replacement time was 7h. After the replacement, the solution was sampled and tested. The contents of platinum, palladium and rhodium in the solution were measured as follows: platinum 4.9ppm, palladium 5.3ppm, rhodium 7.9ppm, and the next step was performed.
[0058] f. Filtration 2: After the replacement is completed, the filtrate is filtered and washed to obtain the filtrate L2 and the filter residue S2. The filter residue S2 is dried and weighed to be 28.3g. The contents of platinum, palladium and rhodium are: platinum 0.81%, palladium 5.78%, rhodium 0.70%, and the enrichment multiple of precious metals is 35 times.
[0059] Example 3
[0060] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0061] a. Crushing: Using the above-mentioned crushed 80 mesh three-way catalyst powder;
[0062] b. Fenton oxidation activation: put 1kg of material powder into a 10L reactor, add 4L of water, 1.2kgMgCl2 and 300gFeCl2, stir and mix, heat to 60°C, maintain the reaction temperature at 60°C, slowly add hydrogen peroxide and 36% mass fraction hydrochloric acid, the hydrogen peroxide drop acceleration rate is 350mL / h, the hydrochloric acid drop acceleration rate is to keep the solution reaction pH = 2-3, stop adding hydrogen peroxide and hydrochloric acid after 1.5h of activation leaching;
[0063] c. Oxidative leaching: After the activation leaching is completed, add 1000mL of 36% mass fraction hydrochloric acid to the reactor, heat to 80°C, slowly add 300mL of saturated sodium chlorate solution, and oxidatively leach for 1.5h;
[0064] d. Filtration 1: After the oxidation leaching is completed, the filtrate is filtered and washed to obtain a filtrate L1 and a filter residue S1. The leaching rates of platinum, palladium and rhodium precious metals in the filtrate L1 and the filter residue S1 are analyzed and detected: platinum 99.3%, palladium 99.6%, and rhodium 95.8%;
[0065] e. Replacement enrichment: The filtrate L1 was added to a stirring tank, and then 120g of iron powder was added and stirred to replace the precious metals. The replacement time was 6h. After the replacement, the solution was sampled and tested. The contents of platinum, palladium and rhodium in the solution were measured as follows: platinum 5.6ppm, palladium 4.8ppm, rhodium 7.5ppm, and the next step was performed.
[0066] f. Filtration 2: After the replacement is completed, the filtrate is filtered and washed to obtain the filtrate L2 and the filter residue S2. The filter residue S2 is dried and weighed to be 21.8g. The contents of platinum, palladium and rhodium are: platinum 1.05%, palladium 7.51%, rhodium 0.90%, and the enrichment multiple of precious metals is 45 times.
[0067] Comparative Example 1
[0068] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0069] a. Crushing: Using the above-mentioned crushed 80 mesh three-way catalyst powder;
[0070] b. Oxidative leaching: put 1kg of material powder into a 10L reactor, add 500mL of 36% mass fraction hydrochloric acid to the reactor, heat to 80°C, slowly add 200mL of saturated sodium chlorate solution, and oxidatively leach for 1h;
[0071] c. Filtration 1: After the oxidation leaching is completed, the filtrate is filtered and washed to obtain a filtrate L1 and a filter residue S1. The leaching rates of platinum, palladium and rhodium precious metals in the filtrate L1 and the filter residue S1 are analyzed and detected: platinum 96.3%, palladium 97.1%, and rhodium 90.3%;
[0072] d. Replacement enrichment: The filtrate L1 was added to a stirring tank, and then 80 g of iron powder was added and stirred to replace the precious metals. The replacement time was 6 h. After the replacement, the solution was sampled and tested. The contents of platinum, palladium and rhodium in the solution were measured as follows: platinum 6.1 ppm, palladium 5.3 ppm, rhodium 9.2 ppm, and the next step was performed.
[0073] e. Filtration 2: After the replacement is completed, filter and wash to obtain the filtrate L2 and the filter residue S2. The filter residue S2 is dried and weighed to be 20.3g. The contents of platinum, palladium and rhodium are: platinum 0.97%, palladium 4.92%, rhodium 0.81%, and the enrichment multiple of precious metals is 21 times.
[0074] Comparative Example 2
[0075] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0076] a. Crushing: Using the above-mentioned crushed 80 mesh three-way catalyst powder;
[0077] b. Fenton oxidation activation: put 1kg of material powder into a 10L reactor, add 4L of water, 1kg of MgCl2 and 200g of FeCl2, stir and mix, heat to 60°C and maintain the temperature, slowly add hydrogen peroxide and 36% mass fraction hydrochloric acid, the hydrogen peroxide drop acceleration rate is 50mL / h, the hydrochloric acid drop acceleration rate is to keep the solution reaction pH = 2-3, and stop adding hydrogen peroxide and hydrochloric acid after 1.5h of activation leaching;
[0078] c. Oxidative leaching: After the activation leaching is completed, add 500mL of 36% mass fraction hydrochloric acid to the reactor, heat to 80°C, slowly add 200mL of saturated sodium chlorate solution, and oxidatively leach for 1h;
[0079] d. Filtration 1: After the oxidation leaching is completed, the filtrate is filtered and washed to obtain a filtrate L1 and a filter residue S1. The leaching rates of platinum, palladium and rhodium precious metals in the filtrate L1 and the filter residue S1 are analyzed and detected: platinum 97.2%, palladium 98.9%, and rhodium 93.2%;
[0080] e. Replacement enrichment: The filtrate L1 was added to a stirring tank, and then 80g of iron powder was added and stirred to replace the precious metals. The replacement time was 6h. After the replacement, the solution was sampled and tested. The contents of platinum, palladium and rhodium in the solution were measured as follows: platinum 5.1ppm, palladium 7.9ppm, rhodium 8.9ppm, and the next step was performed.
[0081] f. Filtration 2: After the replacement is completed, the filtrate is filtered and washed to obtain the filtrate L2 and the filter residue S2. The filter residue S2 is dried and weighed to be 15.4g. The contents of platinum, palladium and rhodium are: platinum 1.01%, palladium 6.85%, rhodium 0.8%, and the enrichment multiple of precious metals is 25 times.
[0082] Comparative Example 3
[0083] A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst comprises the following steps:
[0084] a. Crushing: Using the above-mentioned crushed 80 mesh three-way catalyst powder;
[0085] b. Fenton oxidation activation: 1 kg of material powder was put into a 10 L reactor, and then 4 L of water, 1 kg of MgCl2 and 200 g of FeCl2 were added and stirred, heated to 60 ° C and maintained at this temperature, and hydrogen peroxide and 36% mass fraction of hydrochloric acid were slowly added dropwise, the hydrogen peroxide drop rate was 150 mL / h, and the hydrochloric acid drop rate was to keep the solution reaction pH = 5-7. After 1.5 hours of activation leaching, the addition of hydrogen peroxide and hydrochloric acid was stopped;
[0086] c. Oxidative leaching: After the activation leaching is completed, add 500mL of 36% mass fraction hydrochloric acid to the reactor, heat to 80°C, slowly add 200mL of saturated sodium chlorate solution, and oxidatively leach for 1h;
[0087] d. Filtration 1: After the oxidation leaching is completed, the filtrate L1 and the filter residue S1 are obtained by filtering and washing. The leaching rates of platinum, palladium and rhodium precious metals in the filtrate L1 and the filter residue S1 are analyzed and detected: platinum 68.2%, palladium 65%, and rhodium 60.2%;
[0088] e. Replacement enrichment: The filtrate L1 was added to a stirring tank, and then 80 g of iron powder was added and stirred to replace the precious metals. The replacement time was 6 h. After the replacement, the solution was sampled and tested. The contents of platinum, palladium and rhodium in the solution were measured as follows: platinum 10 ppm, palladium 15 ppm, rhodium 23.2 ppm, and the next step was performed.
[0089] f. Filtration 2: After the replacement is completed, the filtrate is filtered and washed to obtain the filtrate L2 and the filter residue S2. The filter residue S2 is dried and weighed to be 15.3g. The contents of platinum, palladium and rhodium are: platinum 0.71%, palladium 4.5%, rhodium 0.53%, and the enrichment multiple of precious metals is 13 times.
[0090] The leaching rate and recovery rate data of the above embodiments and comparative examples are shown in Table 2 below.
[0091] Table 2:
[0092]
[0093]
[0094] It can be seen from Table 2 above that the overall leaching rate and recovery rate of Examples 1-3 are better than those of Comparative Examples 1-3. Among them, Comparative Example 1 lacks the Fenton oxidation activation step compared to Example 1, and the leaching rates of platinum, palladium, and rhodium are lower than those in Example 1, so the recovery rate is also lower than that in Example 1; Comparative Example 2, compared to Example 1, has too low a hydrogen peroxide droplet acceleration rate, and the Fenton oxidation activation is insufficient, which also makes the leaching rate and recovery rate of precious metals platinum, palladium, and rhodium not good enough; Comparative Example 3, compared to Example 1, has a solution reaction pH of 5-7, which is too high to cause divalent iron precipitation, resulting in a poor Fenton reaction effect, so that the leaching rate and recovery rate of platinum, palladium, and rhodium are low.
[0095] The present invention improves the activity of precious metals by setting Fenton oxidation activation, thereby improving the wet leaching rate and recovery rate of precious metals, and the Fenton oxidation activation step and the oxidation leaching step are completed in the same reactor, shortening the process flow. The filter residue obtained by the first filtration is a mixture of catalyst carrier aluminum oxide and silicon oxide, which can be sold to create economic benefits. The filtrate obtained by the first filtration has a small amount of enriched slag after iron replacement and a high enrichment multiple, which is convenient for subsequent platinum palladium rhodium separation and purification, and there is no problem of difficult treatment of ferrosilicon alloys of pyrometallurgical enrichment. The filtrate obtained by the second filtration is the replacement wastewater, which can be recycled to the Fenton oxidation activation step after adjusting the pH, as shown in Example 2, to reduce wastewater discharge in the process, which is green and environmentally friendly. The equipment used in the whole process is simple, with the advantages of low investment and low energy consumption.
[0096] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst, characterized in that: The steps include: a. Crushing: crushing the ternary waste catalyst into powder; b. Fenton oxidation activation: Add the material and auxiliary materials into the reactor in a mass ratio of material: water: MgCl2: FeCl2 = 1:4:1-2:0.2-1, stir and mix, heat to 50-90°C and maintain, slowly drop hydrogen peroxide and 36% mass fraction hydrochloric acid, and activate leaching for 1-3h; c. Oxidative leaching: After the activation leaching is completed, add 36% mass fraction hydrochloric acid to the reactor, slowly add saturated sodium chlorate solution at 70-80°C, and oxidatively leach for 1-2 hours; d. Filtration 1: After the oxidation leaching is completed, filtration and washing are performed to obtain a filtrate L1 and a residue S1; e. Replacement enrichment: The filtrate L1 is added to a stirring tank, and then iron powder or iron block is added to stir and replace the precious metal. The replacement time is 1-8h. After the replacement, the solution is sampled to detect the residual amount of precious metals and proceed to the next step; f. Filtration 2: After the replacement is completed, filter and wash to obtain the filtrate L2 and the filter residue S2.
2. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: In step a, the ternary waste catalyst is crushed into 40-100 mesh powder.
3. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: In step b, the volume of hydrogen peroxide added dropwise per hour is 0.5-2 times the mass value of FeCl2.
4. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: In step b, hydrochloric acid is slowly added dropwise to maintain the pH of the entire reaction system at 1.5-4.
5. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: The volume of hydrochloric acid in step c is 0.5-2 times the mass value of the material.
6. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: The volume of the saturated sodium chlorate solution in step c is 0.1-1 times the mass value of the material.
7. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: In step e, the amount of iron powder or iron block added is excessive.
8. The method for wet enrichment of platinum, palladium and rhodium from automobile ternary waste catalyst according to claim 1, characterized in that: The step g is also included for the replacement tail liquid reuse: magnesium oxide is added to the filtrate L2, and the pH is adjusted to be greater than 1, and then the solution is returned to the step b for recycling.
Citation Information
Patent Citations
Method for recovering platinum group metal from waste three-way catalyst
CN112442600A
Method for recycling rare and noble metals from waste three-way catalyst
CN113215405A
Method for recovering precious metal from spent automobile catalyst
CN113564379A
Method for recovering palladium, platinum and rhodium from precious iron produced by pyrogenic smelting of automobile waste three-way catalyst
CN117721306A
Process for the recovery of platinum from spent platinum-containing solid residues
WO2023209105A1
Cited By
Method and system for detecting contents of platinum, palladium and rhodium in automobile exhaust purification catalyst and application
CN120801292A