Production method of net-shaped hard alloy

By using ball milling fluid and thermal sintering agonist based on mesh graphene modification in cemented carbide, the problem of degradation of wear resistance and thermal conductivity when improving fracture toughness is solved, and the problem of significantly improving the wear resistance and thermal conductivity of cemented carbide is solved. The product's bending resistance and impact stability are achieved, and the performance is coordinated and improved.

CN118996291APending Publication Date: 2024-11-22ZHUZHOU XINDA MASCH TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411105253.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing cemented carbide improves fracture toughness, it is easy to lead to a reduction in wear resistance and thermal conductivity, and the product's bending resistance and impact stability are insufficient, which limits the use efficiency.

Method used

The mesh cemented carbide production method is adopted, and the ball milling and adjustment liquid based on mesh graphene modification is added to improve the ball milling by combining press molding and spraying heat. Sintering agitator and thermal improvement process coordinate the improvement of fracture toughness, wear resistance and thermal conductivity.

Benefits of technology

The coordinated improvement of the fracture toughness, wear resistance and thermal conductivity of cemented carbide has been achieved, which significantly improves the product's bending resistance and impact stability and improves the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990568140000151
    Figure BDA0004990568140000151
  • Figure BDA0004990568140000161
    Figure BDA0004990568140000161
  • Figure BDA0004990568140000181
    Figure BDA0004990568140000181
Patent Text Reader

Abstract

The invention relates to the technical field of hard alloys, in particular to a production method of a net-shaped hard alloy, which comprises the following steps: weighing the following raw materials in parts by weight: 60-65 parts of tungsten carbide, 10-15 parts of cobalt powder, 0.4-0.7 part of chromium powder, 2-5 parts of nickel powder, 10-15 parts of ball milling effect adjusting liquid based on net-shaped graphene modification and 20-25 parts of hot sintering effect promoting agent. According to the production method of the net-shaped hard alloy, tungsten carbide, cobalt powder, chromium powder and nickel powder are adopted as base materials, and ball milling improvement is carried out by adding ball milling effect adjusting liquid based on net-shaped graphene modification; and the fracture toughness, the wear resistance and the heat-conducting property of the hard alloy obtained by matching with compression molding, spraying of a hot sintering effect promoting agent and a hot improvement process are harmoniously improved, and the bending resistance and impact stability effects of the product are remarkable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cemented carbide, and in particular to a production method of a network-type cemented carbide. Background Art

[0002] Cemented carbide is an alloy material made from hard compounds of refractory metals and bonding metals through a powder metallurgy process. Cemented carbide is widely used as a tool material, such as turning tools, milling cutters, planers, drills, boring tools, etc. It is used to cut cast iron, non-ferrous metals, plastics, chemical fibers, graphite, glass, stone and ordinary steel. It can also be used to cut difficult-to-process materials such as heat-resistant steel, stainless steel, high manganese steel, and tool steel.

[0003] While existing cemented carbides improve fracture toughness, they easily lead to reduced wear resistance and thermal conductivity of the product. The coordinated improvement of fracture toughness, wear resistance and thermal conductivity of the product is the technical difficulty of the present invention. In addition, the product has poor bending resistance and impact stability, which further limits the product's use efficiency. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for producing a network-type cemented carbide to solve the problems raised in the above-mentioned background technology.

[0005] The present invention solves the technical problem by adopting the following technical solution:

[0006] The present invention provides a method for producing a network-type cemented carbide, comprising the following steps:

[0007] Step 1, weighing the raw materials according to weight: 60-65 parts of tungsten carbide, 10-15 parts of cobalt powder, 0.4-0.7 parts of chromium powder, 2-5 parts of nickel powder, 10-15 parts of ball milling conditioning liquid based on network graphene modification and 20-25 parts of thermal sintering accelerator;

[0008] Step 2, tungsten carbide, cobalt powder, chromium powder and nickel powder, and a ball milling conditioning solution modified by mesh graphene are mixed and ball milled at a ball milling speed of 1000-1500 r / min for 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a molding agent;

[0009] Step 3, pressing the molding agent into a mold, and completing the pressing to obtain a molded body;

[0010] Step 4: preheat the molded body to 55-60°C, and then spray the thermal sintering accelerator until the surface of the molded body is soaked;

[0011] Step 5, finally heat improvement treatment, after the treatment is completed, the network type cemented carbide of the present invention can be obtained.

[0012] Preferably, the pressing pressure of the pressing molding is 10-15Mpa, and the pressing time is 1-2h.

[0013] Preferably, the preparation method of the ball-milled conditioning liquid based on the modification of the network graphene is:

[0014] S01: placing the network graphene body in a sufficient amount of 5-7% potassium permanganate solution, stirring and mixing, then washing and drying, and then heat treating at 250-270° C. for 10-15 min. After the treatment is completed, cooling to room temperature to obtain a network graphene activator;

[0015] The preparation method of the network graphene body is as follows:

[0016] A 2 mg / ml graphene oxide solution and a 2 mg / ml nanographene sheet solution were prepared, and the two solutions were ultrasonically mixed, with an ultrasonic power of 350-400 W and an ultrasonic time of 20-30 min, and then hydrothermally reacted at 200° C. for 12 h, and then rinsed with deionized water and dried to obtain a mesh graphene body; wherein the graphene oxide had 10 layers and a lateral size of 50 nm; and the graphene nanosheets had a particle size of 25 μm and 10 layers;

[0017] S02: 3-5 parts of carboxymethyl cellulose, 2-3 parts of sodium lignin sulfonate solution and 2-4 parts of silicon carbide whiskers are mixed thoroughly, and then 1-2 parts of tartaric acid are added and mixed thoroughly to obtain a modified solution;

[0018] The network graphene activator is first immersed in a modification liquid of 3-5 times the total amount of the network graphene activator, and stirred and immersed for treatment, and the stirring and immersion are completed to obtain a modified network graphene agent;

[0019] S03: The modified network graphene agent and the regulating agent are mixed and ball-milled in a weight ratio of 5:3, the ball-milling speed is 1500-1700r / min, the ball-milling is 1-2h, and after the ball-milling is completed, the mixture is washed with water and dried to obtain a regulated and improved network graphene body;

[0020] S04: The modified graphene network, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed in a weight ratio of (3-4):(5-7):1 to obtain a ball-milled conditioning liquid based on modified graphene network.

[0021] Preferably, the mass fraction of the sodium lignin sulfonate solution is 5-8%; the mass fraction of the sodium dodecylbenzene sulfonate solution is 4-6%.

[0022] Preferably, the stirring speed of the stirring immersion treatment is 450-550 r / min, and the stirring time is 30-40 min.

[0023] Preferably, the preparation method of the regulating effect agent is:

[0024] First, add 4-7 parts of boron nitride and 1-3 parts of stearic acid into 5-10 parts of deionized water, stir and disperse evenly, then add 2-4 parts of zirconium oxide and 3-5 parts of yttrium nitrate solution, mix and stir sufficiently, and finally wash with water and dry to obtain the regulating agent.

[0025] Preferably, the mass fraction of the yttrium nitrate solution is 2-5%.

[0026] Preferably, the preparation method of the thermal sintering accelerator is:

[0027] S11: irradiating the lanthanum oxide with protons at a power of 350-400 W for 20-30 min, and obtaining irradiated lanthanum oxide after the irradiation is completed;

[0028] S12: 4-7 parts of irradiated lanthanum oxide, 1-3 parts of ruthenium powder, 3-6 parts of sodium citrate solution, and 1-2 parts of nano-silica sol are mixed and ball-milled at a speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a synergistic agent;

[0029] S13: uniformly mixing the synergist, the silane coupling agent KH560 and the chitosan solution in a weight ratio of 4:1:7 to obtain a thermal sintering accelerator.

[0030] Preferably, the mass fraction of the sodium citrate solution is 4-6%; the mass fraction of the chitosan solution is 2-5%.

[0031] Preferably, the specific operation steps of the thermal improvement treatment are:

[0032] First, heat up to 550℃ at a rate of 2-5℃ / s, keep warm for 1-2h, then heat up to 1050℃ at a rate of 1-3℃ / s, and sinter for 2-3h;

[0033] Then increase the temperature to 1420°C at a rate of 1-2°C / s, continue sintering for 1-2h, and when sintering is complete, cool down to room temperature at a rate of 5-8°C / s.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The production method of the network-type cemented carbide of the present invention uses tungsten carbide, cobalt powder, chromium powder and nickel powder as the base material, and improves the ball milling by adding a ball milling conditioning liquid modified by network graphene, and then cooperates with pressing, spraying a hot sintering accelerator and a thermal improvement process to achieve coordinated improvement in the fracture toughness, wear resistance and thermal conductivity of the cemented carbide, and the product has significant effects on bending resistance and impact stability; the ball milling conditioning liquid modified by network graphene used in the product is used for ball milling improvement, and the hot sintering accelerator is sprayed and the thermal improvement process is used for joint action, and the performance of the product is further improved;

[0036] 2. The ball-milled conditioning liquid based on the modification of the graphene mesh adopts the graphene mesh body through the potassium permanganate solution and the temperature heat treatment of 250-270°C to optimize the activity efficiency of the graphene mesh body. At the same time, the graphene mesh body has a mesh structure, which can support the system products in the system and optimize the system performance effect. After modification by the modifying liquid, the silicon carbide whiskers, sodium lignin sulfonate solution, carboxymethyl cellulose and tartaric acid in the modifying liquid are coordinated and coordinated to work together. The silicon carbide whiskers with whisker-like structure are distributed in the system, and the graphene mesh activator is further coordinated to enhance the performance effect of the system products.

[0037] 3. After the conditioning agent treatment, the conditioning agent is prepared by mixing and stirring boron nitride, stearic acid, zirconium oxide, and yttrium nitrate solution, and the synergistically modified network graphene agent is blended with boron nitride, zirconium oxide, and yttrium nitrate solution to further enhance the fracture toughness, wear resistance, and thermal conductivity of the system to achieve coordinated improvement, and optimize the bending resistance and impact stability of the product. Finally, the sodium dodecylbenzene sulfonate solution and the silane coupling agent KH550 are blended and coordinated, and the raw materials of the system are improved by ball milling to enhance the interface compatibility between the raw materials, so as to better coordinate the ball milling conditioning liquid based on the network graphene modification into the system, thereby enhancing the performance effect of the system;

[0038] 4. The thermal sintering accelerator uses lanthanum oxide to be treated with proton irradiation to activate the active efficiency of lanthanum oxide, and then is treated by ball milling with ruthenium powder, sodium citrate solution and nano-silica sol, and coordinated with lanthanum oxide raw materials, silane coupling agent KH560 and chitosan solution, and then the surface of the molded body is wetted, and after thermal improvement treatment, the thermal sintering accelerator is coordinated with the thermal improvement treatment to further enhance the performance of the product, and the grain structure is refined and activated during the reheating improvement, the density of the tissue is enhanced, and the performance of the product is improved;

[0039] 5. In the thermal improvement treatment, the temperature is raised to 550℃ at a rate of 2-5℃ / s, kept at this temperature for 1-2h, then raised to 1050℃ at a rate of 1-3℃ / s, and sintered for 2-3h; then raised to 1420℃ at a rate of 1-2℃ / s, and sintered for 1-2h. After sintering, the temperature is lowered to room temperature at a rate of 5-8℃ / s. Through continuous temperature rise and sintering improvement, and then cooling treatment, the sintering effect of the organizational structure is optimized and the overall performance of the product is improved. DETAILED DESCRIPTION

[0040] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] A method for producing a network-type cemented carbide in this embodiment comprises the following steps:

[0042] Step 1, weighing the raw materials according to weight: 60-65 parts of tungsten carbide, 10-15 parts of cobalt powder, 0.4-0.7 parts of chromium powder, 2-5 parts of nickel powder, 10-15 parts of ball milling conditioning liquid based on network graphene modification and 20-25 parts of thermal sintering accelerator;

[0043] Step 2, tungsten carbide, cobalt powder, chromium powder and nickel powder, and a ball milling conditioning solution modified by mesh graphene are mixed and ball milled at a ball milling speed of 1000-1500 r / min for 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a molding agent;

[0044] Step 3, pressing the molding agent into a mold, and completing the pressing to obtain a molded body;

[0045] Step 4: preheat the molded body to 55-60°C, and then spray the thermal sintering accelerator until the surface of the molded body is soaked;

[0046] Step 5, finally heat improvement treatment, after the treatment is completed, the network type cemented carbide of the present invention can be obtained.

[0047] The pressing pressure of the pressing molding in this embodiment is 10-15Mpa, and the pressing time is 1-2h.

[0048] The preparation method of the ball-milled conditioning liquid based on the modification of the network graphene in this embodiment is as follows:

[0049] S01: placing the network graphene body in a sufficient amount of 5-7% potassium permanganate solution, stirring and mixing, then washing and drying, and then heat treating at 250-270° C. for 10-15 min. After the treatment is completed, cooling to room temperature to obtain a network graphene activator;

[0050] The preparation method of the network graphene body is as follows:

[0051] A 2 mg / ml graphene oxide solution and a 2 mg / ml nanographene sheet solution were prepared, and the two solutions were ultrasonically mixed, with an ultrasonic power of 350-400 W and an ultrasonic time of 20-30 min, and then hydrothermally reacted at 200° C. for 12 h, and then rinsed with deionized water and dried to obtain a mesh graphene body; wherein the graphene oxide had 10 layers and a lateral size of 50 nm; and the graphene nanosheets had a particle size of 25 μm and 10 layers;

[0052] S02: 3-5 parts of carboxymethyl cellulose, 2-3 parts of sodium lignin sulfonate solution and 2-4 parts of silicon carbide whiskers are mixed thoroughly, and then 1-2 parts of tartaric acid are added and mixed thoroughly to obtain a modified solution;

[0053] The network graphene activator is first immersed in a modification liquid of 3-5 times the total amount of the network graphene activator, and stirred and immersed for treatment, and the stirring and immersion are completed to obtain a modified network graphene agent;

[0054] S03: The modified network graphene agent and the regulating agent are mixed and ball-milled in a weight ratio of 5:3, the ball-milling speed is 1500-1700r / min, the ball-milling is 1-2h, and after the ball-milling is completed, the mixture is washed with water and dried to obtain a regulated and improved network graphene body;

[0055] S04: The modified graphene network, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed in a weight ratio of (3-4):(5-7):1 to obtain a ball-milled conditioning liquid based on modified graphene network.

[0056] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 5-8%; the mass fraction of the sodium dodecylbenzene sulfonate solution is 4-6%.

[0057] The stirring speed of the stirring immersion treatment in this embodiment is 450-550 r / min, and the stirring time is 30-40 min.

[0058] The preparation method of the regulating effect agent of the present embodiment is:

[0059] First, add 4-7 parts of boron nitride and 1-3 parts of stearic acid into 5-10 parts of deionized water, stir and disperse evenly, then add 2-4 parts of zirconium oxide and 3-5 parts of yttrium nitrate solution, mix and stir sufficiently, and finally wash with water and dry to obtain the regulating agent.

[0060] The mass fraction of the yttrium nitrate solution in this embodiment is 2-5%.

[0061] The preparation method of the thermal sintering accelerator of this embodiment is:

[0062] S11: irradiating the lanthanum oxide with protons at a power of 350-400 W for 20-30 min, and obtaining irradiated lanthanum oxide after the irradiation is completed;

[0063] S12: 4-7 parts of irradiated lanthanum oxide, 1-3 parts of ruthenium powder, 3-6 parts of sodium citrate solution, and 1-2 parts of nano-silica sol are mixed and ball-milled at a speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a synergistic agent;

[0064] S13: uniformly mixing the synergist, the silane coupling agent KH560 and the chitosan solution in a weight ratio of 4:1:7 to obtain a thermal sintering accelerator.

[0065] The mass fraction of the sodium citrate solution in this embodiment is 4-6%; the mass fraction of the chitosan solution is 2-5%.

[0066] The specific operation steps of the thermal improvement treatment of this embodiment are:

[0067] First, heat up to 550℃ at a rate of 2-5℃ / s, keep warm for 1-2h, then heat up to 1050℃ at a rate of 1-3℃ / s, and sinter for 2-3h;

[0068] Then increase the temperature to 1420°C at a rate of 1-2°C / s, continue sintering for 1-2h, and when sintering is complete, cool down to room temperature at a rate of 5-8°C / s.

[0069] Example 1.

[0070] A method for producing a network-type cemented carbide in this embodiment comprises the following steps:

[0071] Step 1, weighing the raw materials according to weight: 60 parts of tungsten carbide, 10 parts of cobalt powder, 0.4 parts of chromium powder, 2 parts of nickel powder, 10 parts of ball milling conditioning liquid based on network graphene modification and 20 parts of thermal sintering accelerator;

[0072] Step 2, tungsten carbide, cobalt powder, chromium powder and nickel powder, and a ball milling conditioning solution modified by mesh graphene are mixed and ball milled at a ball milling speed of 1000 r / min for 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a molding agent;

[0073] Step 3, pressing the molding agent into a mold, and completing the pressing to obtain a molded body;

[0074] Step 4: preheat the molded body to 55°C, and then spray the thermal sintering accelerator until the surface of the molded body is wetted;

[0075] Step 5, finally heat improvement treatment, after the treatment is completed, the network type cemented carbide of the present invention can be obtained.

[0076] The pressing pressure of the pressing molding in this embodiment is 10 MPa, and the pressing time is 1 hour.

[0077] The preparation method of the ball-milled conditioning liquid based on the modification of the network graphene in this embodiment is as follows:

[0078] S01: placing the mesh graphene body in a sufficient amount of 5% by mass potassium permanganate solution and stirring and mixing thoroughly, then washing and drying, and then heat treating at 250° C. for 10 min. After the treatment is completed, cooling to room temperature to obtain a mesh graphene activator;

[0079] The preparation method of the network graphene body is as follows:

[0080] A 2 mg / ml graphene oxide solution and a 2 mg / ml nanographene sheet solution were prepared, and the two solutions were ultrasonically mixed, with an ultrasonic power of 350 W and an ultrasonic time of 20 min, and then hydrothermally reacted at 200° C. for 12 h, and then rinsed with deionized water and dried to obtain a mesh graphene body; wherein the graphene oxide had 10 layers and a lateral size of 50 nm; the graphene nanosheets had a particle size of 25 μm and 10 layers;

[0081] S02: 3 parts of carboxymethyl cellulose, 2 parts of sodium lignin sulfonate solution and 2 parts of silicon carbide whiskers are mixed thoroughly, and then 1 part of tartaric acid is added and mixed thoroughly to obtain a modified solution;

[0082] The network graphene activator is first immersed in a modification liquid of 3 times the total amount of the network graphene activator, and stirred and immersed for treatment, and the stirring and immersion are completed to obtain a modified network graphene agent;

[0083] S03: The modified network graphene agent and the regulating agent are mixed in a weight ratio of 5:3 and subjected to ball milling treatment at a ball milling speed of 1500 r / min for 1 h. After the ball milling is completed, the mixture is washed with water and dried to obtain a regulated and improved network graphene body;

[0084] S04: The modified graphene mesh, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed in a weight ratio of 3:5:1 to obtain a ball-milled conditioning liquid based on modified graphene mesh.

[0085] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 5%; the mass fraction of the sodium dodecylbenzene sulfonate solution is 4%.

[0086] The stirring speed of the stirring immersion treatment in this embodiment is 450 r / min, and the stirring time is 30 min.

[0087] The preparation method of the regulating effect agent of the present embodiment is:

[0088] First, add 4 parts of boron nitride and 1 part of stearic acid into 5 parts of deionized water, stir and disperse evenly, then add 2 parts of zirconium oxide and 3 parts of yttrium nitrate solution, mix and stir thoroughly, finally wash with water and dry to obtain the regulating effect agent.

[0089] The mass fraction of the yttrium nitrate solution in this embodiment is 2%.

[0090] The preparation method of the thermal sintering accelerator of this embodiment is:

[0091] S11: irradiating the lanthanum oxide with protons at a power of 350 W for 20 minutes, and then obtaining irradiated lanthanum oxide;

[0092] S12: 4 parts of irradiated lanthanum oxide, 1 part of ruthenium powder, 3 parts of sodium citrate solution and 1 part of nano-silica sol are mixed and ball-milled at a speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a synergistic agent;

[0093] S13: uniformly mixing the synergist, the silane coupling agent KH560 and the chitosan solution in a weight ratio of 4:1:7 to obtain a thermal sintering accelerator.

[0094] The mass fraction of the sodium citrate solution in this embodiment is 4%; the mass fraction of the chitosan solution is 2%.

[0095] The specific operation steps of the thermal improvement treatment of this embodiment are:

[0096] First, heat up to 550°C at a rate of 2°C / s, keep warm for 1h, then heat up to 1050°C at a rate of 1°C / s, and sinter for 2h;

[0097] Then increase the temperature to 1420°C at a rate of 1°C / s, continue sintering for 1h, and when the sintering is completed, cool down to room temperature at a rate of 5°C / s.

[0098] Example 2.

[0099] A method for producing a network-type cemented carbide in this embodiment comprises the following steps:

[0100] Step 1, weighing the raw materials according to weight: 65 parts of tungsten carbide, 15 parts of cobalt powder, 0.7 parts of chromium powder, 5 parts of nickel powder, 15 parts of ball milling conditioning liquid based on network graphene modification and 25 parts of thermal sintering accelerator;

[0101] Step 2, tungsten carbide, cobalt powder, chromium powder and nickel powder, and a ball milling conditioning solution modified by mesh graphene are mixed and ball milled at a ball milling speed of 1500 r / min for 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a molding agent;

[0102] Step 3, pressing the molding agent into a mold, and completing the pressing to obtain a molded body;

[0103] Step 4: preheat the molded body to 60°C, and then spray the thermal sintering accelerator until the surface of the molded body is wetted;

[0104] Step 5, finally heat improvement treatment, after the treatment is completed, the network type cemented carbide of the present invention can be obtained.

[0105] The pressing pressure of the pressing molding in this embodiment is 15Mpa, and the pressing time is 2h.

[0106] The preparation method of the ball-milled conditioning liquid based on the modification of the network graphene in this embodiment is as follows:

[0107] S01: placing the mesh graphene body in a sufficient amount of 7% by mass potassium permanganate solution, stirring and mixing, then washing and drying, and then heat treating at 270° C. for 15 min. After the treatment is completed, cooling to room temperature to obtain a mesh graphene activator;

[0108] The preparation method of the network graphene body is as follows:

[0109] A 2 mg / ml graphene oxide solution and a 2 mg / ml nanographene sheet solution were prepared, and the two solutions were ultrasonically mixed at an ultrasonic power of 400 W for 30 min, and then hydrothermally reacted at 200 ° C for 12 h, and then rinsed with deionized water and dried to obtain a mesh graphene body; wherein the graphene oxide had 10 layers and a lateral size of 50 nm; the graphene nanosheets had a particle size of 25 μm and 10 layers;

[0110] S02: 5 parts of carboxymethyl cellulose, 3 parts of sodium lignin sulfonate solution and 4 parts of silicon carbide whiskers are mixed thoroughly, and then 2 parts of tartaric acid are added and mixed thoroughly to obtain a modified solution;

[0111] The network graphene activator is first immersed in a modification liquid of 5 times the total amount of the network graphene activator, and stirred and immersed for treatment, and the stirring and immersion are completed to obtain a modified network graphene agent;

[0112] S03: The modified network graphene agent and the regulating agent are mixed in a weight ratio of 5:3 and subjected to ball milling treatment at a ball milling speed of 1700 r / min for 2 h. After the ball milling is completed, the mixture is washed with water and dried to obtain a regulated and improved network graphene body;

[0113] S04: The modified graphene network, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed in a weight ratio of 4:7:1 to obtain a ball-milled conditioning solution based on modified graphene network.

[0114] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 8%; the mass fraction of the sodium dodecylbenzene sulfonate solution is 6%.

[0115] The stirring speed of the stirring immersion treatment in this embodiment is 550 r / min, and the stirring time is 40 min.

[0116] The preparation method of the regulating effect agent of the present embodiment is:

[0117] First, add 7 parts of boron nitride and 3 parts of stearic acid into 10 parts of deionized water, stir and disperse them evenly, then add 4 parts of zirconium oxide and 5 parts of yttrium nitrate solution, mix and stir thoroughly, and finally wash with water and dry to obtain the regulating effect agent.

[0118] The mass fraction of the yttrium nitrate solution in this embodiment is 5%.

[0119] The preparation method of the thermal sintering accelerator of this embodiment is:

[0120] S11: irradiating the lanthanum oxide with protons at a power of 400 W for 30 minutes, and then obtaining irradiated lanthanum oxide;

[0121] S12: 7 parts of irradiated lanthanum oxide, 3 parts of ruthenium powder, 6 parts of sodium citrate solution and 2 parts of nano-silica sol are mixed and ball-milled at a speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a synergistic agent;

[0122] S13: uniformly mixing the synergist, the silane coupling agent KH560 and the chitosan solution in a weight ratio of 4:1:7 to obtain a thermal sintering accelerator.

[0123] The mass fraction of the sodium citrate solution in this embodiment is 6%; the mass fraction of the chitosan solution is 5%.

[0124] The specific operation steps of the thermal improvement treatment of this embodiment are:

[0125] First, heat up to 550℃ at a rate of 5℃ / s, keep at this temperature for 2h, then heat up to 1050℃ at a rate of 3℃ / s, and sinter for 3h;

[0126] Then increase the temperature to 1420°C at a rate of 2°C / s and continue sintering for 2 hours. When the sintering is completed, reduce the temperature to room temperature at a rate of 8°C / s.

[0127] Example 3.

[0128] A method for producing a network-type cemented carbide in this embodiment comprises the following steps:

[0129] Step 1, weighing the raw materials according to weight: 62.5 parts of tungsten carbide, 12.5 parts of cobalt powder, 0.55 parts of chromium powder, 3.5 parts of nickel powder, 12.5 parts of ball milling conditioning liquid based on network graphene modification and 22.5 parts of thermal sintering accelerator;

[0130] Step 2, tungsten carbide, cobalt powder, chromium powder and nickel powder, and a ball milling conditioning solution modified by mesh graphene are mixed and ball milled at a ball milling speed of 1250 r / min for 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a molding agent;

[0131] Step 3, pressing the molding agent into a mold, and completing the pressing to obtain a molded body;

[0132] Step 4: preheat the molded body to 57.5°C, and then spray the thermal sintering accelerator until the surface of the molded body is soaked;

[0133] Step 5, finally heat improvement treatment, after the treatment is completed, the network type cemented carbide of the present invention can be obtained.

[0134] The pressing pressure of the pressing molding in this embodiment is 12.5 MPa, and the pressing time is 1.5 h.

[0135] The preparation method of the ball-milled conditioning liquid based on the modification of the network graphene in this embodiment is as follows:

[0136] S01: placing the network graphene body in a sufficient amount of 6% by mass potassium permanganate solution, stirring and mixing, then washing and drying, and then heat treating at 260° C. for 12.5 min. After the treatment is completed, cooling to room temperature to obtain a network graphene activator;

[0137] The preparation method of the network graphene body is as follows:

[0138] A 2 mg / ml graphene oxide solution and a 2 mg / ml nanographene sheet solution were prepared, and the two solutions were ultrasonically mixed, with an ultrasonic power of 375 W and an ultrasonic time of 25 min, and then hydrothermally reacted at 200° C. for 12 h, and then rinsed with deionized water and dried to obtain a mesh graphene body; wherein the graphene oxide had 10 layers and a lateral size of 50 nm; the graphene nanosheets had a particle size of 25 μm and 10 layers;

[0139] S02: 4 parts of carboxymethyl cellulose, 2.5 parts of sodium lignin sulfonate solution and 3 parts of silicon carbide whiskers are mixed thoroughly, and then 1.5 parts of tartaric acid are added and mixed thoroughly to obtain a modified solution;

[0140] The network graphene activator is first immersed in a modification liquid of 4 times the total amount of the network graphene activator, and stirred and immersed for treatment, and the stirring and immersion are completed to obtain a modified network graphene agent;

[0141] S03: The modified network graphene agent and the regulating agent are mixed in a weight ratio of 5:3 and subjected to ball milling treatment at a ball milling speed of 1600 r / min for 1.5 h. After the ball milling is completed, the mixture is washed with water and dried to obtain a regulated and improved network graphene body;

[0142] S04: The modified graphene network, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed in a weight ratio of 5:6:1 to obtain a ball-milled conditioning liquid based on modified graphene network.

[0143] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 6.5%; the mass fraction of the sodium dodecylbenzene sulfonate solution is 5%.

[0144] The stirring speed of the stirring immersion treatment in this embodiment is 500 r / min, and the stirring time is 35 min.

[0145] The preparation method of the regulating effect agent of the present embodiment is:

[0146] First, add 5.5 parts of boron nitride and 2 parts of stearic acid into 7.5 parts of deionized water, stir and disperse them evenly, then add 3 parts of zirconium oxide and 4 parts of yttrium nitrate solution, mix and stir thoroughly, and finally wash with water and dry to obtain the regulating effect agent.

[0147] The mass fraction of the yttrium nitrate solution in this embodiment is 3.5%.

[0148] The preparation method of the thermal sintering accelerator of this embodiment is:

[0149] S11: irradiating lanthanum oxide with protons at a power of 370 W for 25 min, and then obtaining irradiated lanthanum oxide;

[0150] S12: 5.5 parts of irradiated lanthanum oxide, 2 parts of ruthenium powder, 4.5 parts of sodium citrate solution and 1.5 parts of nano-silica sol are mixed and ball-milled at a ball-milling speed of 1250 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a synergistic agent;

[0151] S13: uniformly mixing the synergist, the silane coupling agent KH560 and the chitosan solution in a weight ratio of 4:1:7 to obtain a thermal sintering accelerator.

[0152] The mass fraction of the sodium citrate solution in this embodiment is 5%; the mass fraction of the chitosan solution is 3.5%.

[0153] The specific operation steps of the thermal improvement treatment of this embodiment are:

[0154] First, heat up to 550℃ at a rate of 3.5℃ / s, keep warm for 1.5h, then heat up to 1050℃ at a rate of 2℃ / s, and sinter for 2-3h;

[0155] Then increase the temperature to 1420°C at a rate of 1.5°C / s, continue sintering for 1.5 hours, and end the sintering. Finally, reduce the temperature to room temperature at a rate of 6.5°C / s.

[0156] Comparative Example 1.

[0157] The difference from Example 3 is that the ball milling conditioning liquid modified by network graphene is not added.

[0158] Comparative Example 2.

[0159] The difference from Example 3 is that no modification liquid treatment is used in the preparation of the ball milling conditioning liquid based on the modification of the network graphene.

[0160] Comparative Example 3.

[0161] The difference from Example 3 is that silicon carbide whiskers and tartaric acid are not added to the modified liquid.

[0162] Comparative Example 4.

[0163] The difference from Example 3 is that no conditioning agent is used in the preparation of the ball-milling conditioning liquid based on the modification of the network graphene.

[0164] Comparative Example 5.

[0165] The difference from Example 3 is that SO1 treatment is not used in the preparation of the ball-milled conditioning liquid based on the modification of the network graphene.

[0166] Comparative Example 6.

[0167] The difference from Example 3 is that no thermal sintering accelerator treatment is used.

[0168] Comparative Example 7.

[0169] The difference from Example 3 is that no irradiated lanthanum oxide is added in the preparation of the thermal sintering accelerator.

[0170] Comparative Example 8.

[0171] The difference from Example 3 is that no ruthenium powder or nano-silica sol is added in the preparation of the thermal sintering accelerator.

[0172] Comparative Example 9.

[0173] The difference from Example 3 is that the specific operation steps of the thermal improvement treatment are different:

[0174] Raise the temperature to 1420°C at a rate of 3.5°C / s, sinter for 3 hours, and then cool to room temperature at a rate of 6.5°C / s.

[0175] Comparative Example 10.

[0176] The difference from Example 3 is that the specific operation steps of the thermal improvement treatment are different:

[0177] First, heat up to 550°C at a rate of 3.5°C / s, keep warm for 1.5h, then heat up to 1420°C at a rate of 1.5°C / s, continue sintering for 1.5h, and finally air cool to room temperature after sintering.

[0178] The products of Examples 1 to 3 and Comparative Examples 1 to 10 were subjected to conventional performance tests on fracture toughness, wear resistance (the products were used as cutting tools to cut 42CrMo steel, with a cutting speed of 250m / min, a cutting amount of 2mm, a feed rate of 0.1mm / revolution, and the processing length was completed when the wear of the cutting tool tip reached 0.1mm) and thermal conductivity. The test results are as follows:

[0179]

[0180] The product was treated with 500MP bending strength for 2 minutes, and then 15J / cm 2 The impact toughness was treated for 5 minutes, with the above test as one cycle, and a total of 20 cycles were performed to test the bending resistance and impact resistance stability of the product;

[0181]

[0182] It can be seen from Comparative Examples 1-10 and Examples 1-3 that;

[0183] The product of Example 3 has excellent fracture toughness, and also excellent wear resistance and thermal conductivity. The fracture toughness, wear resistance and thermal conductivity of the product can be improved in a coordinated manner. In addition, the product has excellent bending resistance and impact resistance stability.

[0184] The product did not contain any ball milling conditioning fluid modified by network graphene, and was not treated with a thermal sintering accelerator. The product's performance showed a clear trend of deterioration, and the product's bending resistance and impact resistance stability were significantly deteriorated. The use of ball milling conditioning fluid modified by network graphene and thermal sintering accelerator treatment could improve the product's performance in a coordinated manner, and the product's performance effect was the most significant.

[0185] The performance of the products showed a trend of deterioration when the modified liquid was not treated with the modified liquid, silicon carbide whiskers and tartaric acid were not added to the modified liquid, the modified liquid was not treated with the modified agent, and the modified liquid was not treated with S01. The performance of the products showed a trend of deterioration when the modified liquid obtained by the method of the present invention was combined with the modified agent and S01. The performance of the products showed a trend of deterioration when the modified liquid was combined with the modified agent and S01. The performance of the products showed a trend of deterioration when the modified liquid was combined with the modified agent and S01.

[0186] When no irradiated lanthanum oxide, ruthenium powder or nano-silica sol is added in the preparation of the thermal sintering accelerator, the performance of the product tends to deteriorate. The thermal sintering accelerator obtained by the specific method of the present invention has the most significant product performance effect. Other methods are not as obvious as the effect of the present invention. At the same time, the specific operating steps of the thermal improvement treatment are different, and the performance of the product also tends to deteriorate to varying degrees.

[0187] The present invention further explores the product performance by adjusting the preparation of the effect-enhancing agent;

[0188] Experimental example 1.

[0189] The only difference from Example 3 is that no boron nitride is added in the preparation of the regulating effect agent.

[0190] Experimental example 2.

[0191] The only difference from Example 3 is that zirconium oxide is not added in the preparation of the regulating effect agent.

[0192] Experimental Example 3.

[0193] The only difference from Example 3 is that no yttrium nitrate solution is added during the preparation of the regulating effect agent.

[0194] Experimental Example 4.

[0195] The only difference from Example 3 is that stearic acid is not added in the preparation of the regulating effect agent.

[0196] Taking the above bending resistance and impact resistance stability as the test objects, the effects of the regulating agent on the performance of the product were tested. The test results are as follows;

[0197]

[0198] It can be seen from Experimental Examples 1-4 that when boron nitride is not added in the preparation of the regulating effect agent, the performance of the product changes. In the preparation of the regulating effect agent, the performance deterioration is most obvious, followed by the absence of zirconium oxide. At the same time, when yttrium nitrate solution and stearic acid are not added in the preparation of the regulating effect agent, the performance of the product tends to deteriorate. The regulating effect agents obtained by different methods have different degrees of deterioration in performance. Only the regulating effect agent obtained by the specific method of the present invention has the most significant product performance effect.

[0199] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0200] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for producing a network-type cemented carbide, It is characterized in that The following steps are involved: Step 1, weighing the raw materials according to weight: 60-65 parts of tungsten carbide, 10-15 parts of cobalt powder, 0.4-0.7 parts of chromium powder, 2-5 parts of nickel powder, 10-15 parts of ball milling conditioning liquid based on network graphene modification and 20-25 parts of thermal sintering accelerator; Step 2, tungsten carbide, cobalt powder, chromium powder and nickel powder, and a ball milling conditioning solution modified by mesh graphene are mixed and ball milled at a ball milling speed of 1000-1500 r / min for 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a molding agent; Step 3, pressing the molding agent into a mold, and completing the pressing to obtain a molded body; Step 4: preheat the molded body to 55-60°C, and then spray the thermal sintering accelerator until the surface of the molded body is soaked; Step 5, finally heat improvement treatment, after the treatment is completed, the network type cemented carbide of the present invention can be obtained.

2. A method for producing a network-type cemented carbide according to claim 1, It is characterized in that The pressing pressure of the pressing molding is 10-15Mpa, and the pressing time is 1-2h.

3. A method for producing a network-type cemented carbide according to claim 1, It is characterized in that The preparation method of the ball-milling conditioning liquid based on the modification of the network graphene is as follows: S01: placing the network graphene body in a sufficient amount of 5-7% potassium permanganate solution, stirring and mixing, then washing and drying, and then heat treating at 250-270° C. for 10-15 min. After the treatment is completed, cooling to room temperature to obtain a network graphene activator; The preparation method of the network graphene body is as follows: A 2 mg / ml graphene oxide solution and a 2 mg / ml nanographene sheet solution were prepared, and the two solutions were ultrasonically mixed, with an ultrasonic power of 350-400 W and an ultrasonic time of 20-30 min, and then hydrothermally reacted at 200° C. for 12 h, and then rinsed with deionized water and dried to obtain a mesh graphene body; wherein the graphene oxide had 10 layers and a lateral size of 50 nm; and the graphene nanosheets had a particle size of 25 μm and 10 layers; S02: 3-5 parts of carboxymethyl cellulose, 2-3 parts of sodium lignin sulfonate solution and 2-4 parts of silicon carbide whiskers are mixed thoroughly, and then 1-2 parts of tartaric acid are added and mixed thoroughly to obtain a modified solution; The network graphene activator is first immersed in a modification liquid of 3-5 times the total amount of the network graphene activator, and stirred and immersed for treatment, and the stirring and immersion are completed to obtain a modified network graphene agent; S03: The modified network graphene agent and the regulating agent are mixed and ball-milled in a weight ratio of 5:3, the ball-milling speed is 1500-1700r / min, the ball-milling is 1-2h, and after the ball-milling is completed, the mixture is washed with water and dried to obtain a regulated and improved network graphene body; S04: The modified graphene network, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed in a weight ratio of (3-4):(5-7):1 to obtain a ball-milled conditioning liquid based on modified graphene network.

4. A method for producing a network-type cemented carbide according to claim 3, It is characterized in that The mass fraction of the sodium lignin sulfonate solution is 5-8%; the mass fraction of the sodium dodecylbenzene sulfonate solution is 4-6%.

5. A method for producing a network-type cemented carbide according to claim 3, It is characterized in that The stirring speed of the stirring immersion treatment is 450-550 r / min, and the stirring time is 30-40 min.

6. A method for producing a network-type cemented carbide according to claim 3, It is characterized in that The preparation method of the regulating effect agent is: First, add 4-7 parts of boron nitride and 1-3 parts of stearic acid into 5-10 parts of deionized water, stir and disperse evenly, then add 2-4 parts of zirconium oxide and 3-5 parts of yttrium nitrate solution, mix and stir sufficiently, and finally wash with water and dry to obtain the regulating agent.

7. A method for producing a network-type cemented carbide according to claim 6, It is characterized in that The mass fraction of the yttrium nitrate solution is 2-5%.

8. A method for producing a network-type cemented carbide according to claim 1, It is characterized in that The preparation method of the thermal sintering accelerator is as follows: S11: irradiating the lanthanum oxide with protons at a power of 350-400 W for 20-30 min, and obtaining irradiated lanthanum oxide after the irradiation is completed; S12: 4-7 parts of irradiated lanthanum oxide, 1-3 parts of ruthenium powder, 3-6 parts of sodium citrate solution, and 1-2 parts of nano-silica sol are mixed and ball-milled at a speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a synergistic agent; S13: uniformly mixing the synergist, the silane coupling agent KH560 and the chitosan solution in a weight ratio of 4:1:7 to obtain a thermal sintering accelerator.

9. A method for producing a network-type cemented carbide according to claim 8, It is characterized in that The mass fraction of the sodium citrate solution is 4-6%; the mass fraction of the chitosan solution is 2-5%.

10. The method for producing a network-type cemented carbide according to claim 1, It is characterized in that The specific operation steps of the thermal improvement treatment are: First, heat up to 550℃ at a rate of 2-5℃ / s, keep warm for 1-2h, then heat up to 1050℃ at a rate of 1-3℃ / s, and sinter for 2-3h; Then increase the temperature to 1420°C at a rate of 1-2°C / s, continue sintering for 1-2h, and when sintering is complete, cool down to room temperature at a rate of 5-8°C / s.

Citation Information

Cited By

  • Hard alloy cutter and preparation method thereof

    CN120041736A

  • Hard alloy bearing for hard rock deep drilling and preparation method thereof

    CN120572007A

  • A cemented carbide bearing for hard rock deep drilling and a method for manufacturing the same

    CN120572007B