ErDx preparation method based on magnetron sputtering and product

CN118996355AActive Publication Date: 2024-11-22SICHUAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411094877.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-11
Publication Date
2024-11-22
Estimated Expiration
2044-08-11

AI Technical Summary

Technical Problem

[0005]本发明的目的旨在针对现有技术中制备ErDx效率低、无法实现更高氘含量化合物制备的问题,提供一种基于磁控溅射的ErDx制备方法,能够提高ErDx的制备效率,且通过控制气体流量比和溅射电源电流实现高氘含量

Benefits of technology

[0018] (1) The present invention is based on magnetron sputtering technology. By controlling the gas flow and sputtering power supply control parameters, the deuterium content in the deuteride can be increased, which is conducive to increasing the nuclear reaction yield per unit time;

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996355A_ABST
    Figure CN118996355A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of material preparation, and discloses an ErDx preparation method based on magnetron sputtering and a product, the ErDx preparation method based on magnetron sputtering comprises the following steps: vacuumizing 2 vacuum of magnetron sputtering equipment to be lower than 2 * 10 <-3 > Pa, and then introducing Ar gas; under the condition of Ar gas, pre-sputtering is conducted on the erbium target; after the pre-sputtering is finished, the total air pressure of the Ar gas and the D2 gas is controlled to be 0.3-1.0 Pa, and the flow ratio of the D2 gas to the Ar gas is 2: 3-4: 3; and controlling a sputtering power supply to sputter the erbium target until the ErDx on the substrate reaches a set thickness, thereby obtaining the ErDx film. Based on the magnetron sputtering technology, preparation of ErDx can be achieved by controlling the gas flow and the sputtering power, the deuterium content in the deuteride can be increased, the oxygen content is greatly reduced, the preparation efficiency is improved, and the method is suitable for being used and popularized in the field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation and relates to ErD x Preparation, in particular, involves an ErD based on magnetron sputtering x Preparation method and product. Background Art

[0002] In the past few decades, Erbium Deuteride (ErD x As an important nuclear material, ErD2 is widely used as a target material for neutron generators due to its strong hydrogen storage capacity and good thermal stability. In the diagnostic systems of inertial confinement fusion (ICF) devices such as NIF (National Ignition Facility), OMEGA, and Z, ErD2 is the most commonly used proton source target material for the calibration of proton diagnostic systems. 3 He beam bombardment of ErD x The target material produces calibration protons. The study found that ErD x Deuterium content, bulk oxidation, and thermal stability greatly affect the nuclear reaction rate. Obviously, improving and controlling ErD x The D content in is a relatively important process.

[0003] ErD2 thin film target preparation often uses a two-step method, including erbium film preparation and deuterium loading. In the first step, electron beam evaporation of erbium film is used. In order to eliminate the problems of cracks and peeling of erbium film, the erbium film evaporation rate is generally controlled to 10nm / min; the second step of deuterium loading mainly includes two methods: non-air exposure loading or air exposure loading. Provo et al. published the history of very thick films and bulk samples of group IIIB, IVB, VB and rare earth materials for various vacuum applications. It is mentioned that it takes a total of 84 hours to produce a 50um deuterated erbium film. Such a long time is required to obtain a non-peeling film, but the more complicated process and the long time spent on each step undoubtedly lead to a decrease in production efficiency [see Provo, James L. History of very thick film and bulk sample group IIIB, IVB, VB, and rare earth materials for various vacuum applications. Journal of Vacuum Science & Technology A36.4 (2018)]. The problem with the two-step method is that there are oxides on the surface of the prepared erbium film, which makes it difficult for deuterium atoms to enter the erbium film to form deuterated erbium, greatly slowing down the deuteration rate. Although the increased thermal activation process increases the reaction rate, it also causes more oxygen to enter the body, causing the deuterium atoms in the Er lattice to be replaced by oxygen atoms, which undoubtedly greatly reduces the nuclear reaction rate.

[0004] Adams et al. studied the microstructure, phase formation and stress of reactively-deposited metal hydride films by ion sputtering. They used a Kaufmann ion source to sputter-deposit erbium hydride films in a hydrogen atmosphere. The problem was that when the deposition temperature was below 400°C, there was almost no oxide in the erbium hydride bulk, while slightly more oxygen was found above 400°C [see Adams, David P., et al. Microstructure, phase formation, and stress of reactively-deposited metal hydride thin films. No. SAND 2002-1466. Sandia National Lab. (SNL-NM), Albuquerque, NM (United States); Sandia National Lab. (SNL-CA), Livermore, CA (United States), 2002]. Summary of the invention

[0005] The purpose of the present invention is to prepare ErDx The problem of low efficiency and inability to prepare compounds with higher deuterium content is provided. x Preparation method, capable of increasing ErD x The preparation efficiency is improved, and a high deuterium content is achieved by controlling the gas flow ratio and sputtering power current.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions to achieve it.

[0007] ErD based on magnetron sputtering provided by the present invention x The preparation method comprises the following steps:

[0008] S1 Pump the vacuum of the magnetron sputtering equipment to less than 2×10 -3 Pa, then Ar gas is introduced;

[0009] S2 pre-sputters the erbium target under Ar gas conditions;

[0010] After the S3 pre-sputtering is completed, the total gas pressure of Ar gas and D2 gas is controlled to be 0.3-1.0 Pa, and the flow ratio of D2 gas to Ar gas is 2:3-4:3;

[0011] S4 controls the sputtering power supply to sputter the Erbium target until the ErD on the substrate x Reach the set thickness and get ErD x film; the sputtering power supply is a pulse power supply or a radio frequency power supply; when the sputtering power supply is a pulse power supply, its current is controlled to be 100-500mA, the matching voltage is 300-550V, and the duty cycle is 30%-100%; when the sputtering power supply is a radio frequency power supply, its power is controlled to be 150-300W.

[0012] In the above step S2, the baffle is closed, the Ar gas pressure is controlled to be 0.3-1.0Pa, and the erbium target is pre-sputtered and cleaned for 10-15min; the sputtering power supply is a pulse power supply or a radio frequency power supply; when the sputtering power supply is a pulse power supply, its current is controlled to be 100-500mA, the matching voltage is 300-550V, and the duty cycle is 30%-100%; when the sputtering power supply is a radio frequency power supply, its power is controlled to be 150-300W.

[0013] In the above step S3, the total gas pressure of Ar gas and D2 gas is preferably 0.45-0.6Pa.

[0014] In the above step S2 or S4, when the sputtering power supply is a pulse power supply, the current is preferably 200-300mA, the matching voltage is 360-430V, the duty cycle is preferably 40-60%, and the sputtering time is controlled according to the thickness requirement; when the sputtering power supply is a radio frequency power supply, the sputtering power is preferably 150-200W.

[0015] In the above step S4, the substrate may be Mo or Si; and the distance between the erbium target and the substrate is 8-15 cm.

[0016] The present invention also provides ErD prepared by the above method x Thin film products; the ErD x The x range in the film is 2≤x≤3; ErD x The film thickness can be precisely controlled by the deposition rate. x The film thickness is 3-5 μm. x The oxygen content in the film is very low and the crystal structure is cubic.

[0017] Compared with the prior art, the ErD based on magnetron sputtering provided by the present invention x The preparation method and product have the following beneficial effects:

[0018] (1) The present invention is based on magnetron sputtering technology. By controlling the gas flow rate and sputtering power control parameters, the deuterium content in the deuteride can be increased, which is beneficial to increasing the nuclear reaction yield per unit time;

[0019] (2) The present invention is based on magnetron sputtering technology. By controlling the gas flow rate and sputtering power control parameters, the oxygen content can be greatly reduced to form cubic phase ErD x , which can effectively avoid unnecessary nuclear reaction peaks and deuterium atom diffusion barriers during TDS analysis;

[0020] (3) The present invention is based on magnetron sputtering technology, and ErD is prepared by controlling the gas flow rate and sputtering power control parameters. x The decomposition temperature is high, the performance is stable, and the bonding force with the substrate is strong, which can effectively resist the instability such as target film decomposition and shedding caused by the temperature rise of nuclear reaction (or ion bombardment);

[0021] (4) The present invention is based on magnetron sputtering technology, and ErD can be achieved by controlling the gas flow rate and sputtering power. x The preparation method greatly simplifies the preparation conditions and reduces the preparation time, thereby improving the preparation efficiency and is suitable for popularization and use in this field.

[0022] (5) The present invention is based on magnetron sputtering technology, and the control method of changing the D2 gas flow rate has an effect on the prepared cubic ErD x XRD identification of thin films has unique effects, such as judging ErD2 or ErD3 by the change of preferential deposition of close-packed planes by magnetron sputtering, which is superior to existing technologies. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The Mo-based ErD prepared in Example 1 of the present inventionx Thin film photo (a) and cubic ErD3 lattice structure (b); Er atoms are arranged in a face-centered cubic framework, D O Denotes an octahedral deuterium atom, D T Indicates the tetrahedral occupied deuterium atoms. For the sake of clarity and easy understanding of the picture, the equivalent surface is marked on the crystal plane in Figure (b);

[0024] Figure 2 The Mo-based ErD prepared in Examples 1 to 3 of the present invention x Thin film XRD analysis results;

[0025] Figure 3 The silicon-based ErD prepared in Examples 1 to 3 of the present invention x Thin film SEM analysis results; (a) corresponds to a deuterium gas flow rate of 4 sccm, (b) corresponds to a deuterium gas flow rate of 6 sccm, and (c) corresponds to a deuterium gas flow rate of 8 sccm;

[0026] Figure 4 The Mo-based ErD prepared in Example 1 of the present invention x Thin film EDS analysis results;

[0027] Figure 5 The Mo-based ErD prepared in Examples 1 to 3 of the present invention x Thin film TDS analysis results; (a) is the thermal desorption spectrum, and (b) is the calculated low-temperature peak statistics (the proportion of D atoms occupied by octahedrons). DETAILED DESCRIPTION

[0028] The following will clearly and completely describe the technical solutions of various embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] In this embodiment, Mo and Si are used as substrates respectively, and the distance between the substrate and the erbium target is 10 cm. The radius of the erbium target is 2.5 cm. The sputtering power source used is a pulse power source.

[0031] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0032] S1 pumps the vacuum of the magnetron sputtering equipment to 2×10 -3 Pa, and then Ar gas was introduced.

[0033] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled at 0.45 Pa, the current of the pulse power supply is 200 mA (the matching voltage is 360 V), the duty cycle is 50%, and the cleaning time is 10 minutes.

[0034] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.48 Pa, and the gas flow rate of Ar gas is 6 sccm, and the gas flow rate of D2 gas is 4 sccm.

[0035] The current of the pulse power supply controlled by S4 is 200mA (matching voltage is 360V) and the duty cycle is 50%. The erbium target is sputtered for 45min to obtain ErD deposited on Mo and Si substrates respectively. x film.

[0036] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0037] Example 2

[0038] In this embodiment, Mo and Si are used as substrates respectively, and the distance between the substrate and the erbium target is 10 cm. The radius of the erbium target is 2.5 cm. The sputtering power source used is a pulse power source.

[0039] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0040] S1 pumps the vacuum of the magnetron sputtering equipment to 1.5×10 -3 Pa, and then Ar gas was introduced.

[0041] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled at 0.45 Pa, the current of the pulse power supply is 200 mA (the matching voltage is 360 V), the duty cycle is 50%, and the cleaning time is 10 minutes.

[0042] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.50 Pa, and the gas flow rate of Ar gas is 6 sccm, and the gas flow rate of D2 gas is 6 sccm.

[0043] The current of the pulse power supply controlled by S4 is 200mA (matching voltage is 360V) and the duty cycle is 50%. The erbium target is sputtered for 45min to obtain ErD deposited on Mo and Si substrates respectively. x film.

[0044] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0045] Example 3

[0046] In this embodiment, Mo and Si are used as substrates respectively, and the distance between the substrate and the erbium target is 10 cm. The radius of the erbium target is 2.5 cm. The RF power source used is a pulse power source.

[0047] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0048] S1 pumps the vacuum of the magnetron sputtering equipment to 9×10 -4 Pa, and then Ar gas was introduced.

[0049] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled at 0.45 Pa, the current of the pulse power supply is 200 mA (the matching voltage is 360 V), the duty cycle is 50%, and the cleaning time is 10 minutes.

[0050] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.51 Pa, and the gas flow rate of Ar gas is 6 sccm, and the gas flow rate of D2 gas is 8 sccm.

[0051] The current of the pulse power supply controlled by S4 is 200mA (matching voltage is 360V) and the duty cycle is 50%. The erbium target is sputtered for 45min to obtain ErD deposited on Mo and Si substrates respectively. x film.

[0052] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0053] Example 4

[0054] In this embodiment, Mo and Si are used as substrates respectively, and the distance between the substrate and the erbium target is 10 cm. The radius of the erbium target is 2.5 cm. The sputtering power source used is a pulse power source.

[0055] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0056] S1 pumps the vacuum of the magnetron sputtering equipment to 1×10 -3 Pa, and then Ar gas was introduced.

[0057] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled to 1Pa, the current of the pulse power supply is 100mA (the matching voltage is 300V), the duty cycle is 60%, and the cleaning time is 10min.

[0058] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.47 Pa, and the gas flow rate of Ar gas is 6 sccm, and the gas flow rate of D2 gas is 8 sccm.

[0059] The current of the pulse power supply controlled by S4 is 100mA (the matching voltage is 300V) and the duty cycle is 60%. The erbium target is sputtered for 60min to obtain ErD deposited on Mo and Si substrates respectively. x film.

[0060] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0061] Example 5

[0062] In this embodiment, Mo and Si are used as substrates respectively, and the distance between the substrate and the erbium target is 15 cm. The radius of the erbium target is 2.5 cm. The power supply used is a pulse power supply.

[0063] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0064] S1 pumps the vacuum of the magnetron sputtering equipment to 1×10 -3 Pa conditions, and then Ar gas was introduced.

[0065] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled to be 1Pa, the current of the pulse power supply is 500mA (the matching voltage is 550V), the duty cycle is 100%, and the cleaning time is 10min.

[0066] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 1 Pa, and the gas flow rate of Ar gas is 8 sccm, and the gas flow rate of D2 gas is 8 sccm.

[0067] S4 controls the pulse power supply current to 500mA (matching voltage is 550V) and the duty cycle to 100%. In this case of 100% duty cycle, the pulse power supply is used as a DC power supply. The erbium target is sputtered for 30 minutes to obtain ErD deposited on Mo and Si substrates respectively. x This means that the preparation method of the DC power supply is included.

[0068] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0069] Example 6

[0070] In this embodiment, Mo and Si are used as substrates respectively, and the distance between the substrate and the erbium target is 10 cm. The radius of the erbium target is 2.5 cm. The power supply used is a pulse power supply.

[0071] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0072] S1 pumps the vacuum of the magnetron sputtering equipment to 1×10 -3 Pa conditions, and then Ar gas was introduced.

[0073] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled at 0.3 Pa, the current of the pulse power supply is 300 mA (the matching voltage is 430 V), the duty cycle is 40%, and the cleaning time is 10 minutes.

[0074] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.45 Pa, and the gas flow rate of Ar gas is 6 sccm, and the gas flow rate of D2 gas is 6 sccm.

[0075] The current of the pulse power supply controlled by S4 is 300mA (matching voltage is 430V) and the duty cycle is 40%. The erbium target is sputtered for 30min to obtain ErD deposited on Mo and Si substrates respectively. x film.

[0076] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0077] Example 7

[0078] In this embodiment, Si is used as the substrate, and the distance between the Si substrate and the erbium target is 8 cm. The radius of the erbium target is 2.5 cm. The sputtering power source used is a radio frequency power source.

[0079] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0080] S1 pumps the vacuum of the magnetron sputtering equipment to 2×10 -4 Pa, and then Ar gas was introduced.

[0081] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled at 0.3 Pa, the power of the RF power supply is 150 W, and the cleaning time is 15 minutes.

[0082] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.3 Pa, and the gas flow rate of D2 gas is 5 sccm, and the gas flow rate of Ar gas is 5 sccm.

[0083] S4 controls the power of the RF power supply to 150W, sputters the erbium target for 60 minutes, and obtains ErD deposited on the Si substrate. x film.

[0084] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0085] Example 8

[0086] In this embodiment, Mo is used as the substrate, and the distance between the Mo substrate and the erbium target is 10 cm. The radius of the erbium target is 2.5 cm. The power source used is a radio frequency power source.

[0087] The ErD based on magnetron sputtering provided in this embodiment x The preparation method comprises the following steps:

[0088] S1 pumps the vacuum of the magnetron sputtering equipment to 2×10 -4 Pa, and then Ar gas was introduced.

[0089] The S2 baffle is closed, and the erbium target is pre-sputtered and cleaned. The pre-sputtering conditions are: the Ar gas pressure is controlled at 0.45 Pa, the power of the RF power supply is 300 W, and the cleaning time is 15 minutes.

[0090] After the S3 pre-sputtering is completed, the baffle is opened, and the total gas pressure of Ar gas and D2 gas is controlled to be 0.5 Pa, the gas flow rate of Ar gas is 6 sccm, and the gas flow rate of D2 gas is 8 sccm.

[0091] S4 controls the power of the RF power supply to 300W, sputters the erbium target for 60 minutes, and obtains ErD deposited on the Mo substrate. x film.

[0092] After sputtering, the prepared ErD x The film samples were stored in a dry argon atmosphere to slow down the oxidation rate.

[0093] Next, the ErD prepared in Examples 1-3 above is x The film was subjected to structural and compositional analysis.

[0094] (I) Sample photos and crystal structures

[0095] Mo-based ErD prepared in Example 1 x The photos of the film samples are as follows Figure 1 (a), the crystal structure of ErD3 is shown in Figure 1 (b), where Er atoms are arranged in a face-centered cubic framework, D O Denotes an octahedral deuterium atom, D Trepresents a tetrahedral occupied deuterium atom.

[0096] from Figure 1 (a) It can be seen that the prepared ErD x The film is blue and has a uniform and smooth appearance. Figure 1 (b) It can be seen that in the face-centered cubic framework composed of Er atoms, ErD3 contains all octahedral and tetrahedral sites, while ErD2 mainly occupies tetrahedral sites. In addition, all D atoms are filled in the equivalent (110) and (220) planes, while the atoms in the (111) plane do not change when changing from ErD2 to ErD3. This feature will have a great impact on the close-packed plane preferential deposition of magnetron sputtering, so ErD2 and ErD3 can be roughly distinguished by XRD testing.

[0097] (ii) XRD analysis

[0098] The ErD prepared in Examples 1-3 x The film was subjected to XRD analysis, and the analysis results were as follows Figure 2 shown.

[0099] from Figure 2 It can be seen that when the D2 gas flow rate is 4sccm, the hexagonal Er crystal plane in the film disappears, and the (111) plane maintains a certain height because its atomic density is not much different from (220), which means that all the sputtered Er atoms are converted into ErD2 in the deuterium atmosphere. When the D2 gas flow rate is 6sccm and 8sccm, with the continued increase of D in the (220) plane, the close-packed plane (220) becomes the preferred deposition direction of magnetron sputtering, causing the (111) peak to decrease rapidly and disappear when ErD3 is formed. This can roughly determine the formation of ErD2 and ErD3.

[0100] (III) SEM analysis

[0101] The Si-based ErD prepared in Examples 1-3 x The film was subjected to SEM analysis, and the analysis results were as follows Figure 3 shown.

[0102] from Figure 3 It can be seen that the ErD prepared when the deuterium gas flow rate is 4sccm, 6sccm, and 8sccm x The film thickness is about 3.7-4.2 μm; the film is composed of a typical columnar crystal structure of magnetron sputtering.

[0103] (IV) EDS analysis

[0104] Figure 4 This is a typical surface EDS element analysis. The ErD prepared in Examples 1 to 3 xThe oxygen atoms in the film samples accounted for 6.01%, 3.38% and 3.90% respectively. Note that EDS cannot measure D atoms, so the total number of atoms does not include D atoms when calculating the atomic ratio. Considering that the characterization work is not carried out in situ, the oxygen in the film samples may come from air exposure oxidation or from differences between different samples. However, compared with the general existing technology (thermal diffusion deuteration technology of Er), this is already a very low oxidation level.

[0105] (V) Thermal desorption TDS analysis results

[0106] Figure 5 (a) is the thermal desorption spectrum of the three samples. It can be seen from the figure that the low temperature peak Peak1 is distributed in the range of 400-450℃, and the high temperature peak Peak2 is concentrated around 790℃. The ion current signal can be calibrated and ErD can be measured by the standard leak hole. x The film thickness is used to calculate the atomic ratio of D and Er. The results show that the ErD prepared when the deuterium gas flow rate is 4sccm, 6sccm, and 8sccm x The D / Er atomic ratios of the films were 2:1, 2.5:1, and 3:1, respectively, and the peak area ratios of the low-temperature peak and the high-temperature peak also basically conformed to the standard octahedral and tetrahedral occupancy ratios. These results were consistent with XRD analysis, revealing for the first time the occupancy of deuterium atoms in cubic erbium deuteride deposited by sputtering without temperature control.

[0107] In summary, the ErD developed by the present invention x The overall quality of the film is high, and the preparation method is convenient and effective, which is of great significance for accelerator targets.

[0108] Those skilled in the art will appreciate that the embodiments herein are intended to help readers understand the principles of the present invention, and should be understood that the protection scope of the present invention is not limited to such specific statements and embodiments. Those skilled in the art can make various other specific variations and combinations based on the technical revelations disclosed in the present invention without departing from the essence of the present invention, such as appropriately adjusting the sputtering current or power according to the size of the Er target used, or adjusting the pre-sputtering conditions that do not affect the deposition process, etc., and these variations and combinations are still within the protection scope of the present invention.

Claims

1. ErD based on magnetron sputtering x The preparation method is characterized in that The following steps are involved: S1 Pump the vacuum of the magnetron sputtering equipment to less than 2×10 -3 Pa, then Ar gas is introduced; S2 pre-sputters the erbium target under Ar gas conditions; After the S3 pre-sputtering is completed, the total gas pressure of Ar gas and D2 gas is controlled to be 0.3-1.0 Pa, and the flow ratio of D2 gas to Ar gas is 2:3-4:3; S4 controls the sputtering power supply to sputter the Erbium target until the ErD on the substrate x Reach the set thickness and get ErD x film; the sputtering power supply is a pulse power supply or a radio frequency power supply; when the sputtering power supply is a pulse power supply, its current is controlled to be 100-500mA, the matching voltage is 300-550V, and the duty cycle is 30%-100%; when the sputtering power supply is a radio frequency power supply, its power is controlled to be 150-300W.

2. ErD based on magnetron sputtering according to claim 1 x The preparation method is characterized in that In step S2, the baffle is closed, the Ar gas pressure is controlled to be 0.3-1.0Pa, and the erbium target is pre-sputtered and cleaned for 10-15min; the sputtering power supply is a pulse power supply or a radio frequency power supply; when the sputtering power supply is a pulse power supply, its current is controlled to be 100-500mA, the matching voltage is 300-550V, and the duty cycle is 30%-100%; when the sputtering power supply is a radio frequency power supply, its power is controlled to be 150-300W.

3. ErD based on magnetron sputtering according to claim 1 x The preparation method is characterized in that In step S3, the total gas pressure of Ar gas and D2 gas is 0.45-0.6Pa.

4. ErD based on magnetron sputtering according to claim 1 or 2 x The preparation method is characterized in that The current of the pulse power supply is 200-300mA, the matching voltage is 360-430V, and the duty cycle is 40-60%.

5. ErD based on magnetron sputtering according to claim 1 x The preparation method is characterized in that The power of the radio frequency power supply is 150-200W.

6. ErD based on magnetron sputtering according to claim 1 x The preparation method is characterized in that The substrate is Mo or Si; the distance between the erbium target and the substrate is 8-15 cm.

7. ErD prepared by the method according to any one of claims 1 to 6 x Thin film products.

8. The ErD according to claim 7 x The film product is characterized in that The ErD x The range of x in the film is 2≤x≤3.

9. The ErD according to claim 7 x The film product is characterized in that E x The film thickness is 3-5μm.

Citation Information

Patent Citations

  • Preparation method for deuterium-containing metal film target

    CN106544628A

  • Composite deuterium storage coating for neutron emission tube and preparation method of composite deuterium storage coating

    CN116065122A

  • Graphene modified high-entropy alloy neutron target and preparation method thereof

    CN118335362A