Pretreatment method of scanning electron microscope magnetic powder sample
Through ultrasonic low-temperature dispersion method and conductive resin embedding technology, the poor dispersion and drifting of magnetic powder under scanning electron microscopy are solved, and efficient sample fixation and observation effects are achieved, simplifying the sample preparation process.
Patent Information
- Application Number
- CN202411162430.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
AI Technical Summary
Magnetic powders are prone to interfere with the electron beam during scanning electron microscopy observation, resulting in imaging distortion. Due to magnetic properties and small particle size, it is difficult to stabilize and fix, making it easy to damage the precision components of the electron microscope, and poor dispersion, resulting in poor observation effect.
Ultrasonic low-temperature dispersion is used to form a magnetic powder suspension, which is transferred using a sheet-like carrier and embedded in a conductive resin. Combined with demagnetization treatment, it ensures uniform dispersion and fixation of the powder.
It effectively solves the poor dispersion and drift problems of magnetic powder, improves the observation clarity and accuracy of samples under scanning electron microscope, and simplifies the sample preparation process.
Smart Images

Figure CN119000755A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of scanning electron microscope sample preparation, and in particular relates to a pretreatment method for a scanning electron microscope magnetic powder sample. Background Art
[0002] When observing magnetic powders by scanning electron microscope, the magnetic field of the magnetic powders will interfere with the electron beam of the scanning electron microscope, resulting in image distortion. More importantly, the magnetic powders are easily adsorbed by the strong magnetic field in the scanning electron microscope, especially when the sample is close to the electron beam focusing area of the electron microscope, this adsorption will damage the precision parts of the electron microscope. In addition, due to the small size and magnetic properties of the magnetic powders, it is difficult to ensure their stability using traditional conductive glue or sample stage fixing methods. Under the irradiation of the electron beam, the conductive glue shrinks, causing the magnetic powder particles to drift and affect the observation effect. In addition, the dispersion uniformity of the magnetic powder is also one of the key factors in observing the microscopic morphology and component distribution of the powder. On the one hand, due to the magnetic interaction between the powders, it is difficult to achieve completely uniform dispersion. On the other hand, due to the large specific surface area and high surface energy of the magnetic powders, when their dispersion increases, the free energy of the system is higher, making it very easy for the magnetic powders to re-agglomerate after dispersion. The uneven dispersion of the powders will lead to agglomerations or blank areas in the image, which is not conducive to the observation of their microscopic morphology. At present, there is no effective method to solve the problem of the difficulty of scanning electron microscope sample preparation for magnetic powder samples. Summary of the invention
[0003] In view of the problem that existing magnetic powders are difficult to prepare for scanning electron microscope samples, the purpose of the present invention is to provide a pretreatment method for magnetic powder samples for scanning electron microscope, which solves the problems that existing magnetic powder samples are difficult to disperse, drift during observation, and even damage the precision parts of the electron microscope by dispersing, transferring, embedding and demagnetizing the magnetic powder.
[0004] Based on the above purpose, the technical solution adopted by the present invention is as follows: The present invention provides a method for pretreating a magnetic powder sample for a scanning electron microscope, comprising the following steps: S1: placing magnetic powder in a dispersant, with the weight ratio of magnetic powder to dispersant being 1:(1000-1500), and preparing a magnetic powder suspension by ultrasonic low-temperature dispersion; S2: taking a sheet-shaped carrier and immersing it in the magnetic powder suspension obtained in step S1, taking it out, and quickly drying it; S3: placing a plane of the sheet carrier dried in step S2 horizontally on the surface of the semi-cured conductive resin, and after the magnetic powder on the surface of the sheet carrier adheres to the surface of the semi-cured conductive resin, taking out the sheet carrier; S4: Continue to add conductive resin to the surface of the conductive resin with the magnetic powder adhered thereto for curing until both layers of conductive resin are completely cured; S5: The cured conductive resin is placed in a demagnetizer for demagnetization. The demagnetized sample can be used for scanning electron microscopy observation.
[0005] The present invention adopts the method of dispersing magnetic powder in an organic solvent, and then subjecting the powder to loading, transferring, embedding with a conductive resin and demagnetization treatment on a sheet carrier, thereby solving the problems of poor dispersibility of magnetic powder, easy agglomeration, difficulty in fixation and difficulty in preparing qualified scanning electron microscope samples due to its magnetism. The present invention has a simple and easy pretreatment method for magnetic powder samples and a good sample preparation effect.
[0006] The present invention uses conductive resin to embed magnetic powder samples, which effectively fixes the magnetic powder samples and improves the conductivity of the magnetic powder samples, reduces or avoids the drift phenomenon of the magnetic powder samples that may occur under electron beam irradiation, and ensures the clarity and accuracy of the morphology observation of the magnetic powder samples under a scanning electron microscope.
[0007] The present invention adjusts the weight ratio of the magnetic powder to the dispersant to 1:(1000-1500) so that the dispersant can fully disperse the magnetic powder and reduce the agglomeration of the powder in the subsequent drying process as much as possible.
[0008] Preferably, the dispersant is ethanol or acetone.
[0009] Based on the characteristics of ethanol and acetone being volatile at low temperatures, they are used as dispersion media for magnetic powders to facilitate subsequent low-temperature rapid drying treatment.
[0010] Preferably, the parameters of ultrasonic low-temperature dispersion are as follows: ultrasonic frequency is 60-100 Hz, ultrasonic treatment time is 10-20 min, and ultrasonic treatment temperature is 0-15°C.
[0011] The present invention adopts ultrasonic dispersion of magnetic powder in dispersant under low temperature and short ultrasonic time conditions, which reduces the volatilization of dispersant and more importantly avoids the reagglomeration of magnetic powder after ultrasonic dispersion, thereby prolonging the dispersion stability time of magnetic powder as much as possible.
[0012] Preferably, the sheet-shaped carrier is a glass sheet or a silicon sheet.
[0013] The surface of the sheet carrier is required to be smooth and flat and have a certain hardness to facilitate the transfer operation. Either a glass sheet or a silicon sheet can be used to completely transfer the magnetic powder attached to its surface.
[0014] Preferably, the drying is low-temperature vacuum drying, the vacuum degree is 0.05-0.2 MPa, the drying temperature is 50° C.-70° C., and the drying time is 5-15 min.
[0015] The present invention adopts low-temperature vacuum rapid drying of a sheet carrier loaded with a magnetic powder sample, improves the vacuum degree, reduces the drying temperature, and shortens the drying time, so as to effectively avoid the accumulation of magnetic powder during the slow drying process. The powder is fixed on the sheet carrier through low-temperature rapid drying to achieve the purpose of uniform dispersion.
[0016] Preferably, the conductive resin is conductive epoxy resin or conductive polyimide resin.
[0017] Conductive epoxy resin and conductive polyimide resin have good conductivity. After the magnetic powder is embedded, there is no need to increase the conductivity through gold spraying or other treatments. While embedding and fixing the magnetic powder, its conductivity is improved, which greatly simplifies the pretreatment process of the magnetic powder and has strong operability.
[0018] Compared with the prior art, the present invention has the following beneficial effects: The present invention disperses magnetic powder in a dispersant to form a suspension, immerses a sheet carrier in the suspension, takes it out and dries it, uses the sheet carrier to dry, fix and transfer the dispersed magnetic powder, and then embeds and fixes it with a conductive resin and performs a demagnetization treatment to complete the pretreatment of the magnetic powder for scanning electron microscope sample preparation. By embedding and fixing the magnetic powder with a conductive resin, the problems of poor dispersibility, easy agglomeration, difficulty in fixation and difficulty in preparing qualified scanning electron microscope samples due to the magnetic property of the magnetic powder are solved. The pretreatment method of the present invention can improve the clarity and accuracy of the scanning electron microscope in observing the morphology of the magnetic powder sample, and the pretreatment process of the magnetic powder sample is simple and easy to implement, and the sample preparation effect is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope photo of the magnetic powder sample after pretreatment in Example 1; Figure 2 This is a scanning electron microscope photograph of the magnetic powder sample after pretreatment in Example 1. DETAILED DESCRIPTION
[0020] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The test methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified. Example 1
[0021] This embodiment takes copper-iron soft magnetic powder as an example to provide a method for pretreating magnetic powder samples for a scanning electron microscope, comprising the following steps: S1: The magnetic powder is placed in anhydrous ethanol, the weight ratio of the magnetic powder to the anhydrous ethanol is 1:1200, and ultrasonic low-temperature dispersion is performed to form a magnetic powder suspension; the parameters of the ultrasonic low-temperature dispersion are as follows: the ultrasonic frequency is 80 Hz, the ultrasonic treatment time is 15 min, and the ultrasonic treatment temperature is 10°C.
[0022] S2: Take a glass sheet and immerse it in the magnetic powder suspension obtained in step S1, then take it out and perform low-temperature rapid vacuum drying at 60°C for 10 minutes with a vacuum degree of 0.1 MPa. The magnetic powder is dispersed and fixed on the glass sheet through low-temperature vacuum rapid drying to avoid powder agglomeration caused by too long drying time.
[0023] S3: Use tweezers or other clamping and fixing tools to place a flat surface of the glass sheet dried in step S2 horizontally on the surface of the semi-cured conductive resin. At this time, the surface of the semi-cured conductive resin has begun to solidify. After the magnetic powder on one side of the glass sheet adheres to the surface of the semi-cured conductive resin, take out the glass sheet to transfer the magnetic powder fixed on the surface of the glass sheet to the surface of the conductive resin.
[0024] S4: Continue to add conductive resin to the surface of the conductive resin with the magnetic powder adhered thereto for curing until both layers of conductive resin are completely cured; the conductive resin uses conductive epoxy resin with silver particles.
[0025] S5: The cured conductive resin is placed in a demagnetizer for demagnetization treatment, and the demagnetized sample is used for scanning electron microscopy observation.
[0026] The copper-iron soft magnetic sample pretreated in this embodiment was observed by scanning electron microscope. Figure 1 As shown, it can be seen that the powder sample has good dispersion uniformity and high resolution, and the morphological characteristics of the powder sample can be clearly observed without drift. Example 2
[0027] This embodiment takes copper-iron soft magnetic powder as an example to provide a method for pretreating magnetic powder samples for a scanning electron microscope, comprising the following steps: S1: placing magnetic powder in anhydrous ethanol, the weight ratio of magnetic powder to anhydrous ethanol is 1:1000, and ultrasonic low-temperature dispersion is performed to form a magnetic powder suspension; the parameters of ultrasonic low-temperature dispersion are as follows: ultrasonic frequency is 100 Hz, ultrasonic treatment time is 10 min, and ultrasonic treatment temperature is 0°C.
[0028] S2: Take a glass sheet and immerse it in the magnetic powder suspension obtained in step S1, then take it out and perform low-temperature rapid vacuum drying at 70°C for 5 minutes with a vacuum degree of 0.05 MPa. The magnetic powder is dispersed and fixed on the glass sheet through low-temperature vacuum rapid drying to avoid powder agglomeration caused by too long drying time.
[0029] S3: Use tweezers or other clamping and fixing tools to place a flat surface of the glass sheet dried in step S2 horizontally on the surface of the semi-cured conductive resin. At this time, the surface of the semi-cured conductive resin has begun to solidify. After the magnetic powder on one side of the glass sheet adheres to the surface of the semi-cured conductive resin, take out the glass sheet to transfer the magnetic powder fixed on the surface of the glass sheet to the surface of the conductive resin.
[0030] S4: Continue to add conductive resin to the surface of the conductive resin with the magnetic powder adhered thereto for curing until both layers of conductive resin are completely cured; the conductive resin uses conductive epoxy resin with silver particles.
[0031] S5: The cured conductive resin is placed in a demagnetizer for demagnetization treatment, and the demagnetized sample is used for scanning electron microscopy observation.
[0032] The copper-iron soft magnetic sample pretreated in this embodiment was observed by scanning electron microscope. Figure 2 As shown, it can be seen that the powder sample has good dispersion uniformity and high resolution, and the morphological characteristics of the powder sample can be clearly observed without drift. Example 3
[0033] The only difference between this embodiment and embodiment 1 is that the weight ratio of the magnetic powder to anhydrous ethanol in step S1 is 1:800, 1:1000, 1:1500, and 1:2000, respectively, and the rest of the parts not mentioned are the same as embodiment 1. By comparing the sample preparation effects of magnetic samples treated differently, it is found that when the weight ratio of the magnetic powder to anhydrous ethanol is 1:800, there is stacking of some powder particles, which is not conducive to observing the morphology thereof; when the weight ratio of the magnetic powder to anhydrous ethanol is 1:2000, the powder is too dispersed and the dispersion uniformity is poor; when the weight ratio of the magnetic powder to the dispersant is 1:(1000-1500), the dispersion uniformity of the powder sample is good, and the morphological characteristics of the powder sample can be clearly observed. Comparative Example 1
[0034] The difference between this comparative example and Example 1 is only the temperature of ultrasound. The temperature of ultrasound treatment is set at 30° C. in this example, and the rest of the parts not mentioned are the same as those in Example 1.
[0035] The sample preparation effect of the magnetic samples after pretreatment in this comparative example was analyzed. The magnetic powder samples pretreated in this comparative example were partially stacked and had poor dispersion, indicating that low-temperature ultrasonic dispersion is more conducive to uniform loading of the magnetic powder suspension on the flaky carrier and avoiding agglomeration of the powder during the subsequent drying process. Example 4
[0036] The difference between this embodiment and embodiment 1 is only the drying parameters. The remaining parts not described are the same as those in embodiment 1. The parameters of low-temperature vacuum drying in this embodiment are shown in Table 1 below.
[0037] Table 1 Sample Vacuum degree / MPa Temperature / ℃ Complete drying time / min Sample 1 0.05 40 20 Sample 2 0.05 50 15 Sample 3 0.2 70 15 Sample 4 0.2 80 11 It can be seen from the parameters in Table 1 that the lower the vacuum degree and the higher the drying temperature, the shorter the drying time of the flake carrier. For the electron microscopy sample preparation effect analysis of samples 1 to 4 after pretreatment with the above parameters, compared with samples 1 and 4, the electron microscopy sample preparation effect of samples 2 and 3 after pretreatment is relatively better, the dispersion uniformity of magnetic powder is good, and the clarity of powder morphology is better. However, some powder particles can be seen stacking in samples 1 and 3, which is speculated to be due to the slightly longer drying time of sample 1 and the slightly higher temperature during the drying process of sample 3, which caused some powder particles to agglomerate during the drying process due to the long drying time or high temperature.
Claims
1. A method for pretreating magnetic powder samples for scanning electron microscopy, characterized in that: The steps include: S1: placing magnetic powder in a dispersant, with the weight ratio of magnetic powder to dispersant being 1:(1000-1500), and preparing a magnetic powder suspension by ultrasonic low-temperature dispersion; S2: taking a sheet-shaped carrier and immersing it in the magnetic powder suspension obtained in step S1, taking it out, and quickly drying it; S3: placing a plane of the sheet carrier dried in step S2 horizontally on the surface of the semi-cured conductive resin, and after the magnetic powder on the surface of the sheet carrier adheres to the surface of the semi-cured conductive resin, taking out the sheet carrier; S4: Continue to add conductive resin to the surface of the conductive resin with the magnetic powder adhered thereto for curing until both layers of conductive resin are completely cured; S5: The cured conductive resin is placed in a demagnetizer for demagnetization. The demagnetized sample can be used for scanning electron microscopy observation.
2. The method for pretreating magnetic powder samples for scanning electron microscopy according to claim 1, characterized in that: The dispersant is ethanol or acetone.
3. The method for pretreating magnetic powder samples for scanning electron microscopy according to claim 1, characterized in that: The parameters of the ultrasonic low-temperature dispersion are as follows: the ultrasonic frequency is 60-100 Hz, the ultrasonic treatment time is 10-20 min, and the ultrasonic treatment temperature is 0-15°C.
4. The method for pretreating magnetic powder samples for scanning electron microscopy according to claim 1, characterized in that: The sheet carrier is a glass sheet or a silicon sheet.
5. The method for pretreating magnetic powder samples for scanning electron microscopy according to claim 1, characterized in that: The drying is low-temperature vacuum drying, the vacuum degree is 0.05-0.2 MPa, the drying temperature is 50° C.-70° C., and the drying time is 5-15 min.
6. The method for pretreating magnetic powder samples for scanning electron microscopy according to claim 1, characterized in that: The conductive resin is conductive epoxy resin or conductive polyimide resin.
Citation Information
Cited By
SEM (scanning electron microscope) test sample preparation and demagnetization integrated device for carbon nanotube powder
CN224189931U