Surface-coated high-voltage sodium ion battery positive electrode material and preparation method thereof
By covering Li2MnO3 on the surface of the positive electrode material of the sodium ion battery, the problem of oxygen reaction of layered transition metal oxides at high voltage is solved, high voltage stable charge and discharge and cycle stability are achieved, and the performance of the battery is improved.
Patent Information
- Application Number
- CN202411154469.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-22
AI Technical Summary
Laminated transition metal oxide positive electrode materials are prone to oxygen reactions at high pressure, resulting in poor circulation performance and structural collapse.
The surface of the positive electrode material of sodium ion battery was coated with Li2MnO3 by one-step sintering method to inhibit oxygen reactions, and form a P2-phase layered transition metal oxide to improve the electrochemical performance of the material.
It achieves stable charging and discharging up to 4.7V, maintaining the structural stability and high cycle stability of the material, while improving the capacity and energy density of the battery.
Smart Images

Figure CN119008906A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a surface-coated high-voltage sodium ion battery positive electrode material and a preparation method thereof. Background Art
[0002] In recent years, sodium-ion batteries, as an emerging stationary energy storage technology, have attracted more and more attention due to their abundant sodium resources and low cost. They are mainly composed of four parts: positive electrode, negative electrode, separator and electrolyte. At present, the most commonly used positive electrode materials are layered transition metal oxides, Prussian blue analogs, polyanions and organic positive electrodes, among which layered transition metal oxides are the main positive electrode materials for commercial sodium-ion batteries.
[0003] Voltage window is one of the key factors affecting the electrochemical performance of sodium-ion batteries. A wider voltage window often means that it can provide more capacity. However, when a certain voltage is reached, the layered oxide will inevitably undergo oxygen reaction. As far as the current research status is concerned, the occurrence of oxygen reaction is not conducive to the material's cycle performance, leading to the attenuation of the high-voltage platform of the material and the collapse of the structure. The study found that Li + The substitution changes the redox reaction of the transition metal, thereby suppressing the oxygen redox reaction that may be triggered. + When occupying the alkali metal layer, Li + It does not participate in the reaction process but acts as a support to maintain the material structure. Summary of the invention
[0004] The purpose of the present invention is to address the problem of poor electrochemical performance of existing sodium-ion layered transition metal oxide positive electrode materials under high pressure. A surface coating technology of a one-step sintering method is used to obtain a positive electrode material with a bulk phase of P2 phase and a surface uniformly coated with Li2MnO3, which effectively suppresses the oxygen reaction problem caused by high pressure of the layered transition metal oxide material and can achieve stable charging and discharging up to 4.7V.
[0005] The above-mentioned object of the invention can be achieved through the following technical solutions.
[0006] In a first aspect, the present application provides a sodium ion battery positive electrode material, wherein the sodium ion positive electrode material comprises a sodium ion layered material, and Li2MnO3 coated on at least a portion of the surface of the sodium ion layered material.
[0007] In some embodiments, the layered transition metal oxide Na xMO2 includes at least one of an O3 type sodium ion layered oxide material, a P2 type sodium ion layered oxide material, and a P2 / O3 composite phase sodium ion layered oxide material. Wherein, M is a transition metal ion Ni 3+ , Fe 3+ , Cu 2+ 、Co 3+ Cr 3+ 、Zn 2+ 、Ti 4+ 、V 5+ , Nb 5+ , Mn 3+ , Mn 4+ One or more of; the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrate, sodium phosphate, sodium fluoride, and sodium hydroxide, and x = 0.7 ± 0.05.
[0008] In some embodiments, the surface material is Li2MnO3, wherein the lithium source is one or more of lithium carbonate, lithium sulfate, lithium nitrate, lithium phosphate, lithium acetate, and lithium hydroxide, and the mass of the lithium source is 10% to 30% of the total mass.
[0009] In a second aspect, the present application provides a method for preparing the sodium ion positive electrode material as described in the first aspect, the preparation method comprising:
[0010] The sodium ion battery layered material precursor and lithium salt are mixed to obtain a premix, and the mixture is calcined to obtain the sodium ion positive electrode material in which the Li2MnO3 material layer is coated with the sodium ion layered material.
[0011] In some embodiments, the method for preparing the sodium ion layered material comprises:
[0012] After the metal source precursor is mixed with the sodium source, a calcination reaction is performed to obtain the sodium ion battery layered material.
[0013] In some embodiments, the metal source precursor includes a metal hydroxide or a metal oxide.
[0014] Optionally, the metal element in the metal source precursor includes at least one of Ni, Fe, Mn, Ti, Zn, Cu, Mg, Zr, Mo and Al.
[0015] In some embodiments, the calcination reaction is carried out at a temperature of 850° C. to 950° C. for 15 hours, and the calcination reaction is carried out in an oxygen atmosphere.
[0016] In a third aspect, the present application provides a battery, wherein the positive electrode material in the battery includes the sodium ion positive electrode material as described in the first aspect.
[0017] Compared with the traditional technology, this application has at least the following beneficial effects:
[0018] The present application adopts Li2MnO3 material to coat the layered transition metal oxide positive electrode material, which not only maintains the cycle stability of the layered transition metal oxide positive electrode material, but also avoids the structural problems caused by the high-pressure oxygen reaction.
[0019] The present invention synthesizes a P2 phase layered transition metal oxide positive electrode material with Li2MnO3 coated on the surface by a one-step sintering method, and the material has excellent electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the XRD pattern of prepared Example 1;
[0021] Figure 2 is the XRD pattern of the prepared comparative example 1;
[0022] Figure 3 The SEM images and mappings of Example 1 and Comparative Example 1 are shown;
[0023] Figure 4 The charge and discharge curve of the sodium ion battery prepared in Example 1 at 2.00-4.70V;
[0024] Figure 5 The charge and discharge curve of the sodium ion battery prepared in Comparative Example 1 at 2.00-4.70V;
[0025] Figure 6 This is a graph showing the cycle performance of the sodium ion battery prepared in Example 1 at 2.00-4.70V;
[0026] Figure 7 This is a graph showing the cycle performance of the sodium ion battery prepared in Comparative Example 1 at 2.00-4.70V; DETAILED DESCRIPTION
[0027] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.
[0028] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.
[0029] The present invention designs a novel positive electrode material for sodium ion batteries, which is coated on the surface of a layered transition metal oxide of a sodium ion battery. In order to better understand the technical content of the present invention, a specific embodiment is given and described as follows in conjunction with the accompanying drawings.
[0030] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.
[0031] The present invention designs a novel positive electrode material for sodium ion batteries. By coating a Li2MnO3 layer on the surface of a layered transition metal oxide for sodium ion batteries, the migration, dissolution and oxygen redox problems of transition metals on the surface of the layered transition metal oxide material are effectively suppressed, thereby obtaining a layered transition metal oxide positive electrode material for sodium ion batteries with high initial efficiency, long cycle and wide voltage window.
[0032] In an exemplary embodiment of the present invention, a sodium-electrode layered transition metal oxide positive electrode material with a surface coated with Li2MnO3 is provided, wherein the bulk phase of the positive electrode material is a layered transition metal oxide Na x MO2 composition, and the surface of the bulk phase has a coating layer uniformly coated with Li2MnO3;
[0033] The layered transition metal oxide is Na x MO2, where M is the transition metal ion Ni 3+ , Fe 3+ , Cu 2+ 、Co 3+ Cr 3+ 、Zn 2+ 、Ti 4+ 、V 5+ , Nb 5+ , Mn 3+ , Mn 4+ One or more of; the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrate, sodium phosphate, sodium fluoride, and sodium hydroxide, and x = 0.7 ± 0.05.
[0034] It should be understood that when M is two or more, the molar ratio between different transition metal ions is not limited, and the molar ratio of the total transition metal ions only needs to be 1.
[0035] By coating the surface of the material to a certain extent, the surface of the material can acquire new physical, chemical and other new functions, thereby greatly improving the dispersion of the material and its compatibility with other substances. Common coating methods mainly include the following categories: mechanical mixing method, solid phase reaction method, hydrothermal method, sol-gel method, precipitation method and deposition method. Among them, solid phase synthesis is the simplest and most convenient, and most suitable for commercialization. When using the solid phase method for surface coating, it is often combined with the sol-gel method or precipitation method, or through secondary sintering. The entire process is relatively cumbersome, and it is easy to have problems such as uneven and loose coating.
[0036] Therefore, in another embodiment of the present invention, a method for preparing the aforementioned sodium-electrode layered transition metal oxide positive electrode material with Li2MnO3 coated on the surface is provided, comprising the following steps:
[0037] A transition metal source, a sodium source, and a lithium source are used as raw materials, and after being uniformly mixed by ball milling according to a stoichiometric ratio, they are heat treated in an air atmosphere and then cooled to obtain a sodium-electrolyte layered transition metal oxide positive electrode material with a surface coated with Li2MnO3. In an optional embodiment, in the transition metal source, the metal element in the metal source precursor includes at least one of Ni, Fe, Mn, Ti, Zn, Cu, Mg, Zr, Mo and Al.
[0038] In an alternative embodiment, the transition metal source is a transition metal salt or a transition metal oxide or a transition metal hydroxide;
[0039] In an optional embodiment, the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrate, sodium phosphate, sodium fluoride, and sodium hydroxide.
[0040] In an optional embodiment, the lithium source is one or more of lithium carbonate, lithium sulfate, lithium nitrate, lithium phosphate, lithium acetate, and lithium hydroxide.
[0041] In an optional embodiment, the mass of the transition metal source and the sodium source is calculated according to the layered transition metal oxide Na x The material is prepared by the stoichiometric ratio of MO2, and the mass of the lithium source is 10% to 30% of the total mass.
[0042] In an optional embodiment, the heat treatment condition is heat treatment at 850-950° C. for 15 hours.
[0043] In an embodiment of the present invention, there is also provided an application of the aforementioned surface-coated sodium-electrode layered transition metal oxide positive electrode material in a sodium ion battery. The surface-coated sodium-electrode layered transition metal oxide positive electrode material exhibits excellent capacity and cycle stability under conditions as high as 4.7V.
[0044] For better understanding, the present invention is further described below in conjunction with specific examples, but the processing technology is not limited thereto, and the content of the present invention is not limited thereto.
[0045] Example 1
[0046] Set 1 mol Na 0.7 Mn 8 / 13 Ni 1 / 13 Ti 1 / 13 Li 3 / 13 O2, Na2CO3, NiO, TiO2, Mn2O3, Li2CO3 according to the molar ratio of Na:Ni:Ti:Mn:Li=0.7:8 / 13:1 / 13:1 / 13:3 / 13 (wherein the Na source is 5% excess), after uniform mixing, heat treatment at 900°C for 15h, and cooling with the furnace to obtain surface-coated layered transition metal oxide powder.
[0047] Example 2
[0048] Set 1 mol Na 0.7 Mn 8 / 13 Ni 1 / 13 Ti 1 / 13 Li 3 / 13 O2, Na2CO3, NiO, TiO2, Mn2O3, Li2CO3 according to the molar ratio of Na:Ni:Ti:Mn:Li=0.7:8 / 13:1 / 13:1 / 13:3 / 13 (wherein the Na source is 5% excess), after mixing evenly, heat treatment at 850°C for 15h, and cooling with the furnace to obtain surface-coated layered transition metal oxide powder.
[0049] Example 3
[0050] Set 1 mol Na 0.7 Mn 8 / 13 Ni 1 / 13 Ti 1 / 13 Li 3 / 13 O, Na2CO3, NiO, TiO2, Mn2O3, Li2CO3 according to the molar ratio of Na:Ni:Ti:Mn:Li=0.7:8 / 13:1 / 13:1 / 13:3 / 13 (wherein the Na source is 5% excess), after uniform mixing, heat treatment at 950°C for 15h, and cooling with the furnace to obtain a surface-coated layered transition metal oxide powder.
[0051] Example 4
[0052] Set 1 mol Na 0.7 Mn 0.8 Ni 0.1 Ti 0.1 Li 0.3O2, Na2CO3, NiO, TiO2, Mn2O3, Li2CO3 according to the molar ratio of Na:Ni:Ti:Mn:Li=0.7:8 / 13:1 / 13:1 / 13:3 / 13 (wherein the Na source is 5% excess), after uniform mixing, heat treatment at 900°C for 15h, and cooling to obtain surface-coated layered transition metal oxide powder.
[0053] Example 5
[0054] Set 1 mol Na 0.7 Mn 0.8 Ni 0.1 Ti 0.1 Li 0.3 O2, Na2CO3, NiO, TiO2, Mn2O3, Li2CO3 according to the molar ratio of Na:Ni:Ti:Mn:Li=0.7:0.8:0.1:0.1:0.3 (wherein the Na source is 5% excess), after mixing evenly, heat treatment at 850°C for 15h, and cooling to obtain a surface-coated layered transition metal oxide powder.
[0055] Example 6
[0056] Set 1 mol Na 0.7 Mn 0.8 Ni 0.1 Ti 0.1 Li 0.3 O2, Na2CO3, NiO, TiO2, Mn2O3, Li2CO3 according to the molar ratio of Na:Ni:Ti:Mn:Li=0.7:0.8:0.1:0.1:0.3 (wherein the Na source is 5% excess), after mixing evenly, heat treatment at 950°C for 15h, and cooling to obtain a surface-coated layered transition metal oxide powder.
[0057] Comparative Example 1
[0058] Set 1 mol Na 0.7 MnO2, Na2CO3, and Mn2O3 are mixed uniformly according to the molar ratio of Na:Mn=0.7:1 (wherein the Na source is 5% in excess), and then heated at 900°C for 15h and cooled in the furnace to obtain a layered transition metal oxide powder.
[0059] XRD
[0060] XRD test was performed on the materials obtained in Examples 1-6 and Comparative Example 1. The results are as follows: Figure 1 and Figure 2 shown.
[0061] The XRD patterns of Examples 2-6 are the same as those of Example 1, which are P2 phase and Li2MnO3 coating layer. The sample of Comparative Example 1 is pure P2 phase.
[0062] SEM
[0063] The materials obtained in Example 1 and Comparative Example 1 were subjected to SEM test, and the results are as follows: Figure 3 and Figure 4 shown.
[0064] It can be seen from the SEM images that the samples of the comparative example and the embodiment are all block materials with uniform element distribution.
[0065] Preparation of electrodes and testing of their electrochemical properties
[0066] The prepared positive electrode material was uniformly mixed with superconducting carbon black (Super P) and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1, and an appropriate amount of N-methylpyrrolidone (NMP) was added to prepare a slurry, which was then coated on a carbon-coated aluminum foil with a thickness of 200 μm, then dried in a vacuum oven at 120°C for 4 hours, and cut into original sheets with a diameter of 12 mm using a cutting machine to obtain the corresponding electrode.
[0067] The above-obtained electrode was used as the positive electrode and the sodium metal sheet as the negative electrode. 1.0M NaClO4 in PC with 2% FEC (NC-005) was selected as the electrolyte. They were assembled into half-cells in an argon atmosphere glove box. The electrochemical properties of each were tested by a Xinwei tester, including specific capacity, cycle stability and first-cycle coulombic efficiency. The test voltage range was 2.0 to 4.7V.
[0068] Compared with Example 1, it can be seen that the sodium ion positive electrode material of the present application not only has a higher first efficiency (the first week coulomb efficiency of Experimental Example 1 is 99%, and that of Comparative Example 1 is 76%), but also obtains a higher specific capacity (the reversible specific capacity of Experimental Example 1 is 163.12 mAh / g, and that of Comparative Example 1 is 134.44 mAh / g). At the same time, due to the protection of the oxide shell, the cycle stability is also greatly improved (the capacity retention rate of Experimental Example 1 after 100 cycles is 98.2%, and the capacity retention rate of Comparative Example 1 after 100 cycles is 66.7%). Therefore, the present application adopts a sodium ion layered material coated with Li2MnO3, which can achieve stable charge and discharge up to 4.7V, maintaining the structural stability of the base material while maintaining the high gram capacity of the sodium ion layered material. Moreover, the positive electrode material of the present application can consume a part of the residual alkali and can remain stable in the electrolyte. During the cycle of the layered material, it can reduce the cycle deterioration caused by the phase change of the material, so that the layered structure inside the material can still be maintained. It has the characteristics of good surface stability, low residual alkali and high gram capacity, thereby improving the battery energy density and cycle performance.
[0069] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A sodium ion positive electrode material, characterized in that: The sodium ion positive electrode material comprises a sodium ion layered material and an oxide coating material layer coated on at least a portion of the surface of the sodium ion layered material.
2. The sodium ion positive electrode material according to claim 1, characterized in that The sodium ion positive electrode material satisfies at least one of the following conditions: (1) The material of the oxide coating material layer includes at least one of Li2MnO3, Li2MnO4, LiMnO, LiMnO2, LiMn2O4, and Li2Mn2O4; (2) The sodium ion layered material includes at least one of a sodium ion O3 type sodium ion layered oxide material, a P2 type sodium ion layered oxide material and a P2 / O3 composite phase sodium ion layered oxide material; optionally, the sodium ion layered material includes at least one of sodium manganate and doped sodium manganate.
3. The sodium ion positive electrode material according to claim 1 or 2, characterized in that The mass of the oxide coating material layer accounts for 10% to 30% of the mass of the sodium ion positive electrode material.
4. A method for preparing the sodium ion positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: The raw materials of the sodium ion layered material and the coated oxide material are mixed to obtain a premix, and the premix is calcined to obtain the sodium ion positive electrode material in which the oxide material layer coats the sodium ion layered material.
5. The preparation method according to claim 4, characterized in that: The preparation method of the sodium ion layered material comprises: After the metal source precursor is mixed with the sodium source, a calcination reaction is performed to obtain the sodium ion layered material.
6. The preparation method according to claim 5, characterized in that: The preparation method of the sodium ion layered material satisfies at least one of the following conditions: (1) The metal source precursor comprises a metal hydroxide or a metal oxide; optionally, the metal element in the metal source precursor comprises at least one of Ni, Fe, Mn, Ti, Zn, Cu, Mg, Zr, Mo and Al; (2) The sodium source is at least one of sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrate, sodium phosphate, sodium fluoride, and sodium hydroxide; (3) The molar ratio of sodium ions in the sodium source to the metal elements in the metal source precursor is (0.67-0.72):1; (4) The calcination reaction is carried out at a temperature of 850° C. to 950° C. for a time of 8 h to 12 h, and the calcination reaction is carried out in an oxygen-containing atmosphere.
7. The preparation method according to claim 4, characterized in that: The raw materials for preparing the oxide coating material include transition metal oxide, lithium source and carbon source; Optionally, the metal element in the transition metal oxide includes at least one of V, Mn, Fe, Cr, Ni, Cu and Zn; Optionally, the lithium source is at least one of lithium carbonate, lithium sulfate, lithium nitrate, lithium phosphate, lithium acetate, and lithium hydroxide; Optionally, the carbon source includes an organic carbon source. Further optionally, the carbon source includes at least one of sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrate, sodium phosphate, sodium fluoride, and sodium hydroxide.
8. The preparation method according to claim 7, characterized in that: The preparation method also satisfies at least one of the following conditions: (1) The molar ratio of the sodium ion layered material to the transition metal oxide is 1:(0-1), but does not include 0; (2) The molar ratio of the sodium ion layered material to the lithium source is 1:(0-1), but does not include 0.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method also satisfies at least one of the following conditions: (1) The mixing method includes ball milling mixing; (2) The calcination temperature is 800° C. to 1000° C., the time is 10 h to 15 h, and the atmosphere is a protective atmosphere; (3) The molar ratio of the sodium ion layered material to the organic carbon source is 1:(0-1), but does not include 0.
10. A battery, characterized in that: The positive electrode material in the battery comprises the sodium ion positive electrode material according to any one of claims 1 to 3.
Citation Information
Cited By
P '2-phase sodium-electrode layered transition metal oxide positive electrode material as well as preparation method and application thereof
CN119612595A
Negative-electrode-free sodium battery positive electrode material as well as synthesis method and application thereof
CN121839637A