Inorganic solid water-based electrolyte and preparation method thereof
By using inorganic solid water-based electrolytes in water-based sodium ion batteries, using materials such as hydrated inorganic salts and flame retardants to form a highly crosslinked structure, the problems of narrow voltage window, low ionic conductivity and poor safety are solved, and the battery is realized Significant improvements in performance and security.
Patent Information
- Application Number
- CN202410953555.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-12-03
AI Technical Summary
The existing water-based sodium ion battery electrolytes have problems such as narrow voltage window, low ion conductivity, poor safety, and insufficient mechanical strength, which limits the performance and safety of the battery.
Using the preparation method of inorganic solid water-based electrolyte, the highly crosslinked solid electrolyte is formed by selecting appropriate hydrated inorganic salts, thickeners and flame retardants, ensuring stability and safety in a wide temperature range and improving ion conduction Rate.
It significantly improves the cycle stability, Coulomb efficiency and safety of the battery, expands the electrochemical window, reduces the volatility and polarity of the electrolyte, and enhances the mechanical strength and leakage prevention capabilities of the battery.
Smart Images

Figure CN119069833A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based sodium battery electrolytes, and in particular to an inorganic solid water-based electrolyte and a preparation method thereof. Background Art
[0002] With the transformation of the automobile industry and the demand for sustainable energy development, lithium-ion batteries dominate the market, but they have shortcomings in terms of safety, cycle life, charge and discharge rate, and environmental protection. As a new energy storage technology, sodium-ion batteries have attracted widespread attention due to their abundant resources, cost advantages, high energy density, and environmental protection. In the field of sodium-ion battery electrolytes, non-aqueous electrolytes are sensitive to trace amounts of water, and some sodium salts have poor solubility; although ionic liquid electrolytes have good stability, they have high viscosity, low ionic conductivity, and high cost.
[0003] The prior art has the following defects:
[0004] 1. The voltage window of water-based electrolyte is narrow, usually below 1.23V, which limits the output voltage and energy density of water-based sodium-ion batteries. Due to its limited voltage window, the range of electrode materials available is limited;
[0005] 2. The ionic conductivity of existing organic solid electrolytes is low. Although the solid phase structure helps prevent electrolyte leakage, it also restricts the movement of ions and affects the performance of the battery.
[0006] 3. In conventional water-based electrolytes, there is a large amount of highly active free water, the electrolyte has a high dissolved oxygen content, the interface stability is poor, and the electrode-electrolyte interface side reaction phenomenon is serious, causing the active material to dissolve and the electrolyte to decompose, thereby limiting the performance of the battery;
[0007] 4. Liquid electrolytes have evaporation and leakage problems, and are less safe. Inorganic solvents generally have poor thermal stability and are extremely flammable, which poses a great risk to battery safety. For example, EC:DMC contains 1M (mol / L) NaPF 6 and NaClO in EC:DMC 4 The electrolytes start to decompose at >75 and 60 °C, respectively, which endangers battery safety;
[0008] 5. Good mechanical strength can inhibit the growth of metal negative electrode dendrites. The mechanical strength of existing solid electrolytes is insufficient, which easily leads to the rupture of the electrolyte layer and the separation between the electrode and the electrolyte;
[0009] In order to solve the problems of easy volatility, high polarity and limited voltage range of traditional water-based electrolytes, the present invention is specially proposed to prepare an inorganic solid water-based electrolyte, which can significantly improve battery performance and cycle life. Summary of the invention
[0010] The purpose of the present invention is to overcome the defects of the prior art and provide an inorganic solid-state water-based electrolyte and a preparation method thereof. The inorganic solid-state water-based electrolyte not only overcomes the shortcomings of traditional electrolytes, but also, due to its unique solid-state properties, remains stable over a wide temperature range, thereby improving the safety and environmental adaptability of the battery, and providing a new option for the application of sodium-ion batteries in the field of sustainable energy.
[0011] The present invention provides the following technical solutions:
[0012] The present invention provides a method for preparing an inorganic solid water-based electrolyte, comprising the following steps:
[0013] S1. Weighing raw materials, wherein the raw materials include a first hydrated inorganic salt, a second hydrated inorganic salt, a thickener and a flame retardant in a mass ratio of (30-40):(150-200):(0.1-5):(2-5), the first hydrated inorganic salt is one of sodium acetate, sodium sulfate, sodium perchlorate or sodium dihydrogen phosphate, the second hydrated inorganic salt is one of acetate, sulfate, sodium perchlorate or sodium dihydrogen phosphate, and the first hydrated inorganic salt and the second hydrated inorganic salt are different substances;
[0014] S2. Using deionized water as the matrix, gradually add the second hydrated inorganic salt to the matrix under stirring, add the first hydrated inorganic salt, flame retardant and thickener after uniform dispersion, continue stirring until uniform, and form a solid mixed electrolyte after standing;
[0015] S3, drying the solid mixed electrolyte obtained in step S2 to remove the excess solvent precipitated from the upper layer, thereby obtaining the inorganic solid water-based electrolyte.
[0016] The hydrated inorganic salt added to the raw material in the present invention is an anhydrous crystalline powder, which can form a hydrated state after being added to water. The first hydrated inorganic salt of the present invention is the main body of the electrolyte, and the second hydrated inorganic salt is used to cause the common ion effect with the first hydrated inorganic salt to reduce the solubility of the solution, and thickeners, flame retardant additives, etc. are added to stabilize the solution, gradually restrict the flow of solvent molecules and make the solution form a solid state, and maintain normal ion conduction during the charge and discharge process, so as to obtain a solidified state of the inorganic solid water-based electrolyte material, thereby achieving supercooling and inhibiting phase separation.
[0017] The prepared inorganic solid water-based electrolyte has an inherent highly cross-linked spatial network structure that keeps it insoluble and forms a stable shape. At room temperature, it appears as a white, opaque waxy product with a high degree of independence and rigidity. It can maintain this shape over a wide temperature range (-30°C-70°C). When the temperature is heated to 80°C and above, the product begins to dissolve into a colorless, transparent, colloidal liquid. It has a series of mechanical properties and liquid properties, but it is different from ordinary solid electrolytes. It is a solid electrolyte formed by inorganic solid substances that can phase change. This structure ensures cohesion, effectively constructs a hydrated inorganic network, promotes the movement of ions in the solution, and effectively improves conductivity.
[0018] Furthermore, the thickener is a mixture of PVA / NaBr or polyacrylic acid, and the mass ratio of PVA:NaBr in the mixture of PVA / NaBr is 6-8:2-4.
[0019] Furthermore, the flame retardant is a phosphate flame retardant, and the phosphate flame retardant is one of trimethyl phosphate, triethyl phosphate, triphenyl phosphate or tricresyl phosphate.
[0020] Furthermore, in step S3, the drying temperature is 40-70° C., and the drying time is 10-90 min.
[0021] The present invention also provides an inorganic solid water-based electrolyte prepared by the above preparation method, wherein the mass ratio of each component in the electrolyte is: 10-14% of the first hydrated inorganic salt, 60-70% of the second hydrated inorganic salt, 0.5-3% of the thickener, 0-1% of the flame retardant, and 15-25% of water.
[0022] The invention also provides application of the inorganic solid water-based electrolyte in a sodium ion battery.
[0023] The present invention has the following beneficial effects:
[0024] 1. The inorganic solid-state water-based electrolyte of the present invention contains almost no free solvent, and the activity of water is significantly suppressed, which inhibits the dissolution of the positive electrode material. The surface defects formed during the charge and discharge process can be repaired in situ, the dissolution balance can be improved, the dissolution rate of transitional sodium ions can be reduced, and the battery cycle stability can be further improved, thereby achieving the characteristics of battery cycle stability and excellent rate performance.
[0025] 2. The inorganic solid water-based electrolyte of the present invention constructs a multi-solute system by introducing a co-solvent with a high solvent donor number to design an antifreeze electrolyte with a low eutectic temperature and strong supercooling ability, thereby realizing a water-based sodium ion battery that can maintain cycle stability even at low temperatures.
[0026] 3. The inorganic solid water-based electrolyte of the present invention has strong toughness and wear resistance, strong mechanical strength such as bonding strength and compression and bending resistance, and anti-leakage ability. Adding the second hydrated inorganic salt can promote the migration of sodium ions and increase its elasticity. In addition, the high-concentration electrolyte system increases the anion reduction potential (higher than the hydrogen evolution potential) due to the increase in salt concentration. A good SEI is formed on the electrode surface before hydrogen evolution in the electrolyte, which can effectively expand the electrochemical window of the water-based electrolyte, thereby improving the performance of the battery, and improving the coulombic efficiency and cycle stability of the battery.
[0027] 4. The inorganic solid water-based electrolyte of the present invention has good flame retardancy and high safety, low preparation cost, simple preparation process and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a picture of the inorganic solid electrolyte prepared in Example 1 of the present invention;
[0030] Figure 2 The charge and discharge curve of the inorganic solid electrolyte prepared in Example 1 of the present invention after being used as an electrolyte for a sodium ion battery;
[0031] Figure 3 The figure is the charge and discharge curve of the electrolyte prepared in the comparative example of the present invention after being used as the electrolyte of the sodium ion battery. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] An embodiment of the present invention provides a method for preparing an inorganic solid water-based electrolyte, comprising the following steps:
[0034] S1. Weighing raw materials, wherein the raw materials include a first hydrated inorganic salt, a second hydrated inorganic salt, a thickener and a flame retardant in a mass ratio of (30-40):(150-200):(0.1-5):(2-5), the first hydrated inorganic salt is one of sodium acetate, sodium sulfate, sodium perchlorate or sodium dihydrogen phosphate, the second hydrated inorganic salt is one of acetate, sulfate, sodium perchlorate or sodium dihydrogen phosphate, and the first hydrated inorganic salt and the second hydrated inorganic salt are different substances;
[0035] S2. Using deionized water as the matrix, gradually add the second hydrated inorganic salt to the matrix under stirring, add the first hydrated inorganic salt, flame retardant and thickener after uniform dispersion, continue stirring until uniform, and form a solid mixed electrolyte after standing;
[0036] S3, drying the solid mixed electrolyte obtained in step S2 to remove the excess solvent precipitated from the upper layer, thereby obtaining the inorganic solid water-based electrolyte.
[0037] The first hydrated inorganic salt is the main body of the electrolyte, and the second hydrated inorganic salt is added to produce the common ion effect with the first hydrated inorganic salt to reduce the solubility of the solution, and thickeners, flame retardant additives, etc. are added to stabilize the solution, gradually restrict the flow of solvent molecules and make the solution form a solid state, and maintain normal ion conduction during the charge and discharge process.
[0038] The second hydrated inorganic salt can effectively inhibit the side reactions of hydrogen and oxygen evolution and improve the coulombic efficiency of the battery. Sodium ions migrate through the liquid phase provided by the second hydrated inorganic salt, and heteroatom-solvated sodium ions are transported through the hydrated inorganic chain movement, which can effectively improve the conductivity of the solid-state battery electrolyte.
[0039] In a specific embodiment, the thickener is a mixture of PVA / NaBr or polyacrylic acid, and the mass ratio of PVA:NaBr in the mixture of PVA / NaBr is 6-8:2-4.
[0040] PVA can improve the conductivity of ions and reduce the activation energy. The ion mixture of the selective ion channel can act as a support to fill the vacancies formed by the Prussian cathode materials during the cycle, which promotes the inhibition of the dissolution and structural distortion of the Prussian cathode and contributes to the cycle stability of the Prussian cathode.
[0041] In a specific embodiment, the flame retardant is a phosphate flame retardant, and the phosphate flame retardant is one of trimethyl phosphate, triethyl phosphate, triphenyl phosphate or tricresyl phosphate.
[0042] There is a synergistic effect between the components of the inorganic solid water-based electrolyte prepared by the present invention. The thickener can reduce the activation energy, improve the electrical conductivity of the ions, improve the electrochemical performance of the battery, and fill the vacancies formed during the cycle, thereby achieving the technical effects of high capacity and stable cycle of the Prussian positive electrode; the addition of the flame retardant greatly enhances the safety characteristics of the electrolyte, and the battery will not catch fire or explode.
[0043] The inorganic solid water-based electrolyte prepared by the present invention has the following mass ratios: 10-14% of the first hydrated inorganic salt, 60-70% of the second hydrated inorganic salt, 0.5-3% of the thickener, 0-1% of the flame retardant, 15-25% of water, and the sodium salt concentration in the electrolyte is 5-10 mol / L.
[0044] The second hydrated organic salt content in the present invention is less than 60%, which is not effective in stabilizing the solid state; the thickener content is too low, which cannot play the role of a support body to fill holes and cannot inhibit Prussian dissolution; the content is too high, which will reach or even exceed the saturation concentration, resulting in precipitation of the electrolyte. The sodium salt concentration is too low, resulting in too low ion conductivity of the electrolyte, affecting battery performance, and too high will increase costs.
[0045] The addition of flame retardants can further reduce the freezing point of the electrolyte. If the mass ratio of flame retardants is too low, it will not have a flame retardant effect, thereby reducing the safety performance of the electrolyte; if the mass ratio is too high, it will not be fully miscible. Experiments have shown that the above mass ratio range is more appropriate.
[0046] In order to better understand the specific implementation scheme of the present invention, this patent is explained below in conjunction with specific examples.
[0047] Example 1
[0048] 1) Weigh 30.0 g of sodium acetate, 150.0 g of potassium acetate, 3 g of polyacrylic acid, and 2.0 g of tricresyl phosphate.
[0049] 2) 50.0g high-purity deionized water is used as a matrix to reduce the impact of impurities on the performance of the electrolyte. Then, under stirring, potassium acetate solid is gradually added to the water to ensure that it is evenly dispersed, and the stirring speed is 200r / min. Subsequently, sodium acetate solid and tricresyl phosphate are added, and stirring is continued until the solution forms a solid state. The above-mentioned solid matter is left to stand at room temperature for 30 minutes to ensure that the mixed components are uniform and stable, and a solid mixed material is obtained (at this time, a clear liquid will be precipitated in the upper layer).
[0050] 3) placing the solid mixed material prepared in step 2) into an oven, and drying the lower solid electrolyte in the oven to remove excess solvent and ensure the formation of a stable solid electrolyte layer, wherein the oven temperature is 50° C. and the heating time is 30 minutes.
[0051] Figure 1 is a photo of the solid electrolyte prepared in Example 1 after thermal curing. The solid electrolyte prepared in this example is a white, opaque, waxy product. Figure 2 The positive electrode material (Prussian blue) and the negative electrode material (hard carbon) were assembled into an aqueous sodium ion battery for battery testing. The overpotential can be maintained at about 1.1V for a long time, the first cycle coulomb efficiency is close to 100%, and the decline is not obvious after 2000 cycles. After the first cycle of charging, the sodium deposition on the surface of the current collector is dense and no sodium dendrites are generated.
[0052] Example 2
[0053] 1) Weigh 30.0 g sodium sulfate, 150.0 g potassium acetate, 2.0 g tricresyl phosphate and 2.0 g PVA / NaBr (7:3).
[0054] 2) Under stirring, solid sodium sulfate is gradually added to 50.0g of water to ensure that it is evenly dispersed, and the stirring speed is 200r / min. Subsequently, solid sodium acetate and tricresyl phosphate are added, and stirring is continued until the solution is uniform. Then, a mixture of PVA / NaBr (7:3) is added in a certain proportion so that its mass accounts for 2%, and continuous stirring is performed to ensure that the additive is completely dissolved and evenly distributed until the solution forms a solid state. The above-mentioned solid material is allowed to stand at room temperature for 30 minutes to ensure that the mixed components are uniform and stable, and a solid mixed material is obtained (clear liquid will precipitate on the upper layer).
[0055] 3) placing the solid mixed material prepared in step 2) into an oven, and drying the lower solid electrolyte in the oven to remove excess solvent and ensure the formation of a stable solid electrolyte layer, wherein the oven temperature is 50° C. and the heating time is 30 minutes.
[0056] The inorganic solid electrolyte prepared in this example is a white, opaque waxy product. The positive electrode material (sodium manganate) and the negative electrode material (titanium phosphate) are assembled into an aqueous sodium ion battery for battery testing. The overpotential can be maintained at about 1V for a long time, the first cycle coulomb efficiency is close to 100%, and there is almost no decrease after 1500 cycles. After the first cycle of battery charging is completed, the sodium deposition on the surface of the current collector is dense, and no sodium dendrites are generated.
[0057] Example 3
[0058] 1) Weigh 30.0 g sodium perchlorate, 200.0 g potassium acetate, 2.0 g tricresyl phosphate and 2.0 g PVA / NaBr (7:3).
[0059] 2) Under stirring, solid potassium acetate is gradually added to 50.0g of water to ensure that it is evenly dispersed, and the stirring speed is 200r / min. Subsequently, solid sodium perchlorate and tricresyl phosphate are added, and stirring is continued until the solution is uniform. Then, a mixture of PVA / NaBr (7:3) is added in a certain proportion so that its mass accounts for 1.8%, and continuous stirring is performed to ensure that the additive is completely dissolved and evenly distributed until the solution forms a solid state. The above-mentioned solid substance is allowed to stand at room temperature for 30 minutes to ensure that the mixed components are uniform and stable, and a solid mixed substance is obtained (clear liquid will precipitate on the upper layer).
[0060] 3) placing the solid mixed material prepared in step 2) into an oven, and drying the lower solid electrolyte in the oven to remove excess solvent and ensure the formation of a stable solid electrolyte layer, wherein the oven temperature is 50° C. and the heating time is 30 minutes.
[0061] The inorganic solid electrolyte prepared in this example is a white, opaque, waxy product. The positive electrode material (Prussian white) and the negative electrode material (sodium titanium phosphate) were assembled into an aqueous sodium ion battery for battery testing, in which the overpotential can be maintained at about 1.1V for a long time, the first cycle coulomb efficiency is close to 100%, and there is almost no decrease after 1200 cycles. After the first cycle of battery charging is completed, the sodium deposition on the surface of the current collector is dense, and no sodium dendrites are generated.
[0062] Example 4
[0063] 1) Weigh 30.0 g of sodium acetate, 200.0 g of sodium dihydrogen phosphate, 2.0 g of tricresyl phosphate and 2.0 g of polyacrylic acid.
[0064] 2) Under stirring, gradually add sodium acetate solid to 50.0g water to ensure that it is evenly dispersed, and the stirring speed is 200r / min. Subsequently, sodium dihydrogen phosphate solid and tricresyl phosphate are added, and stirring is continued until the solution is uniform. Then, polyacrylic acid is added in a certain proportion so that its mass proportion reaches 1.8%, and stirring is continued to ensure that the additive is completely dissolved and evenly distributed until the solution forms a solid state. The above-mentioned solid material is allowed to stand at room temperature for 30 minutes to ensure that the mixed components are uniform and stable, and a solid mixed material is obtained (clear liquid will precipitate on the upper layer).
[0065] 3) placing the solid mixed material prepared in step 2) into an oven, and drying the lower solid electrolyte in the oven to remove excess solvent and ensure the formation of a stable solid electrolyte layer, wherein the oven temperature is 50° C. and the heating time is 30 minutes.
[0066] The inorganic solid electrolyte prepared in this example is a white, opaque, waxy product. The positive electrode material (manganese dioxide) and the negative electrode material (sodium titanium phosphate) were assembled into an aqueous sodium ion battery for battery testing, in which the overpotential can be maintained at about 1.1V for a long time, the first cycle coulomb efficiency is close to 100%, and there is almost no decrease after 800 cycles. After the first cycle of battery charging is completed, the sodium deposition on the surface of the current collector is dense, and no sodium dendrites are generated.
[0067] Example 5
[0068] 1) Weigh 30.0 g of sodium sulfate, 150.0 g of sodium dihydrogen phosphate, 2.0 g of tricresyl phosphate and 2.0 g of polyacrylic acid.
[0069] 2) Under stirring, solid potassium acetate is gradually added to 50.0g of water to ensure that it is evenly dispersed, and the stirring speed is 200r / min. Subsequently, solid sodium perchlorate and tricresyl phosphate are added, and stirring is continued until the solution is uniform. Then, a mixture of polyacrylic acid is added in a certain proportion so that its mass accounts for 1.8%, and continuous stirring is performed to ensure that the additive is completely dissolved and evenly distributed until the solution forms a solid state. The above-mentioned solid material is allowed to stand at room temperature for 30 minutes to ensure that the mixed components are uniform and stable, and a solid mixed material is obtained (clear liquid will precipitate out on the upper layer).
[0070] 3) placing the solid mixed material prepared in step 2) into an oven, and drying the lower solid electrolyte in the oven to remove excess solvent and ensure the formation of a stable solid electrolyte layer, wherein the oven temperature is 50° C. and the heating time is 30 minutes.
[0071] The inorganic solid electrolyte prepared in this example is a white, opaque waxy product. The positive electrode material (sodium iron pyrophosphate) and the negative electrode material (Prussian blue) are assembled into an aqueous sodium ion battery for battery testing, in which the overpotential can be maintained at about 1.1V for a long time, the first cycle coulomb efficiency is close to 100%, and there is almost no decrease after 1200 cycles. After the first cycle of battery charging is completed, the sodium deposition on the surface of the current collector is dense, and no sodium dendrites are generated.
[0072] Comparative Example 1
[0073] 1) Weigh 30.0 g sodium sulfate, 2.0 g tricresyl phosphate and 2.0 g PVA / NaBr (7:3).
[0074] 2) Under stirring, gradually add potassium sulfate solid to 50.0g of water to ensure that it is evenly dispersed, and the stirring speed is 200r / min. Subsequently, add tricresyl phosphate and continue stirring until the solution is uniform. Then, add a mixture of PVA / NaBr (7:3) in a certain proportion so that its mass ratio reaches 1.8%, heat to 50 degrees and continue stirring to ensure that the additive is completely dissolved and evenly distributed. The mixed solution is allowed to stand at room temperature for 30 minutes, and crystals are precipitated from the solution.
[0075] 3) Put the mixed electrolyte solution prepared in step 2) into an oven, and dry the lower solid electrolyte in the oven to remove excess solvent. The oven temperature is 50° C. and the heating time is 30 minutes.
[0076] In this comparative example, no solid electrolyte is produced, and the electrolyte solution is still in liquid state. Figure 3 , the battery test was carried out by assembling water-based positive electrode materials and water-based negative electrode materials into aqueous sodium-ion batteries, in which the overpotential can be maintained at about 1.3V for a long time, and the first cycle coulomb efficiency is close to 57%. It dropped significantly after 100 cycles. After the first cycle of charging, the sodium deposition on the surface of the current collector was obviously dense, and sodium dendrites were generated. It can be seen that if the second hydrated inorganic salt is not added, it will be difficult to form an inorganic solid electrolyte, and hydrogen and oxygen evolution reactions in the aqueous battery environment will easily occur, affecting the normal charge and discharge of the battery and greatly reducing the cycle stability of the battery.
[0077] The inorganic solid electrolyte prepared in the embodiment of the present invention was also subjected to low temperature performance test (freezing test in -20°C environment) and flame retardant performance test. The electrolyte did not freeze at -20°C, which verified its good low temperature performance. The electrolyte would not spontaneously combust or explode under high temperature or short circuit conditions, which greatly improved the safety of the battery.
[0078] The inorganic solid water-based electrolyte of the present invention has significant advantages in component ratio and preparation method, and can effectively improve the low temperature performance, electrochemical performance and safety of the battery. Experimental data prove the high efficiency and stability of the patented electrolyte in practical applications. The inorganic solid water-based electrolyte provides new ideas and technical support for the development and application of solid-state batteries through its unique temperature adaptability, efficient ion conduction mechanism and optimized formula design.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an inorganic solid water-based electrolyte, characterized in that: The following steps are involved: S1. Weighing raw materials, wherein the raw materials include a first hydrated inorganic salt, a second hydrated inorganic salt, a thickener and a flame retardant in a mass ratio of (30-40):(150-200):(0.1-5):(2-5), the first hydrated inorganic salt is one of sodium acetate, sodium sulfate, sodium perchlorate or sodium dihydrogen phosphate, the second hydrated inorganic salt is one of acetate, sulfate, sodium perchlorate or sodium dihydrogen phosphate, and the first hydrated inorganic salt and the second hydrated inorganic salt are different substances; S2. Using deionized water as the matrix, gradually add the second hydrated inorganic salt to the matrix under stirring, add the first hydrated inorganic salt, flame retardant and thickener after uniform dispersion, continue stirring until uniform, and form a solid mixed electrolyte after standing; S3, drying the solid mixed electrolyte obtained in step S2 to remove the excess solvent precipitated from the upper layer, thereby obtaining the inorganic solid water-based electrolyte.
2. The method for preparing an inorganic solid water-based electrolyte according to claim 1, characterized in that: The thickener is a mixture of PVA / NaBr or polyacrylic acid, and the mass ratio of PVA:NaBr in the mixture of PVA / NaBr is 6-8:2-4.
3. The method for preparing an inorganic solid water-based electrolyte according to claim 1, characterized in that: The flame retardant is a phosphate flame retardant, and the phosphate flame retardant is one of trimethyl phosphate, triethyl phosphate, triphenyl phosphate or tricresyl phosphate.
4. The method for preparing an inorganic solid water-based electrolyte according to claim 1, characterized in that: In step S3, the drying temperature is 40-70° C., and the drying time is 10-90 min.
5. An inorganic solid water-based electrolyte prepared by the preparation method according to any one of claims 1 to 4.
6. The inorganic solid water-based electrolyte according to claim 5, characterized in that: The mass ratio of each component in the electrolyte is: 10-14% of the first hydrated inorganic salt, 60-70% of the second hydrated inorganic salt, 0.5-3% of the thickener, 0-1% of the flame retardant, and 15-25% of water. The sodium salt concentration in the electrolyte is 5-10 mol / L.
7. Use of the inorganic solid water-based electrolyte according to claim 5 in sodium ion batteries.