Preparation method of silicon-carbon negative electrode material, silicon-carbon negative electrode material and lithium battery
By preparing silicon carbon anode material, using three-dimensional porous carbon skeleton and prelithiation reaction, the volume effect and interface side reaction problems of silicon anode material in lithium-ion batteries are solved, and the battery performance and safety are improved.
Patent Information
- Application Number
- CN202411188989.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
Silicon negative electrode materials have volume effects and serious interface side effects in lithium-ion batteries, resulting in degradation of battery performance and safety issues.
Using the preparation method of silicon-carbon negative electrode material, a silicon-carbon mixture is formed by pre-forming a solution of silicon and carbon sources, and a silicon-oxycarbon composite on a three-dimensional porous carbon framework is formed during freeze-drying and calcining, followed by molten lithium. The metal is prelithiated to form a solid electrolyte interface film containing lithium oxide.
Effectively alleviate volume effects, reduce interface side reactions, and improve the overall performance and safety of lithium batteries.
Smart Images

Figure CN119008907A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a method for preparing a silicon-carbon negative electrode material, a silicon-carbon negative electrode material and a lithium battery. Background Art
[0002] Lithium battery is a type of battery with lithium as its main component. It includes two major categories: lithium metal battery and lithium ion battery. Among them, the most common and widely used is the lithium ion battery, which is mainly composed of a positive electrode, a negative electrode, an electrolyte and a separator. The working principle is the embedding and de-embedding between the positive and negative electrodes to achieve the storage and release of electrical energy.
[0003] In the relevant lithium-ion battery preparation technology, graphite is often used as anode material due to its stable electrochemical performance and low operating voltage. However, the theoretical specific capacity of graphite anode is only 372mAh / g, which is close to its limit and difficult to meet the demand for higher energy density.
[0004] Silicon has a theoretical specific capacity of up to 4200mAh / g and a moderate operating voltage (Li 4.4 Si is considered the most likely material to replace graphite anode. However, silicon anode has significant volume effect during charge and discharge (forming Li 4.4 Si), resulting in particle fragmentation, loss of electrical contact with the current collector, and severe interface side reactions. In order to alleviate the volume effect of silicon anode, researchers have developed silicon composite materials with larger specific surface area, which further aggravates the interface side reactions.
[0005] Current silicon negative electrode materials have problems such as volume effect and serious interface side reactions, which not only reduce the overall performance of lithium-ion batteries, but also easily affect the safety of lithium-ion batteries. Summary of the invention
[0006] The present application provides a method for preparing a silicon-carbon negative electrode material, a silicon-carbon negative electrode material and a lithium battery, so as to solve or partially solve the problem of how to improve the overall performance and safety of lithium batteries when using silicon as the negative electrode material of the battery.
[0007] The first aspect of the present application provides a method for preparing a silicon-carbon negative electrode material, comprising: Pre-preparing a first solution and a second solution; Evenly mixing the first solution and the second solution to obtain a silicon-carbon mixed solution; Adding a sacrificial template to the silicon-carbon mixed solution and mixing them evenly to obtain a precursor solution, and freeze-drying the precursor solution to obtain a precursor; The precursor is subjected to calcination and carbonization and sample treatment to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton; The silicon-oxygen-carbon composite is added into molten lithium metal to carry out a pre-lithiation reaction, thereby obtaining a silicon-carbon negative electrode material containing a solid electrolyte interface film of lithium oxide.
[0008] Optionally, the pre-preparing of the first solution and the second solution comprises: dissolving a silicon source into an aqueous ammonia solution to obtain the first solution; dissolving a carbon source in deionized water to obtain the second solution; Wherein, the silicon source is one of silicon monoxide and silicon dioxide, and the carbon source is one of glucose, polyacrylonitrile and polyvinyl pyrrolidone.
[0009] Optionally, the first solution and the second solution are mixed evenly to obtain a silicon-carbon mixed solution, comprising: The second solution is added dropwise into the first solution, and after mixing evenly, the silicon-carbon mixed solution is obtained.
[0010] Optionally, the sacrificial template is sodium chloride, and the sacrificial template is added to the silicon-carbon mixed solution and mixed evenly to obtain a precursor solution, comprising: Adding the sodium chloride into the silicon-carbon mixed solution and mixing them evenly to obtain the precursor solution; The freeze-drying of the precursor solution to obtain the precursor comprises: The precursor solution is transferred to a freeze dryer, and the precursor solution is heated from the starting temperature to room temperature according to a preset temperature increase gradient and temperature increase rate, and maintained at each temperature stage for a period of time until the water content of the precursor solution is completely sublimated to obtain the precursor.
[0011] Optionally, the starting temperature is -50°C, the temperature rising gradient is 10°C, the temperature rising rate is 8°C / min-12°C / min, and the holding time of each temperature stage is 2h-6h.
[0012] Optionally, the sample treatment includes washing, filtering and drying, and the precursor is subjected to calcination, carbonization and sample treatment to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton, including: The precursor is calcined and carbonized under a protective atmosphere to convert the silicon source into silicon oxide and the carbon source into carbon; the carbon and the silicon oxide are coated on the surface of the sacrificial template; The calcined and carbonized precursor is washed, filtered and dried with deionized water to remove the sacrificial template, thereby obtaining a silicon-oxygen-carbon composite in which silicon and oxygen are covered on the three-dimensional porous carbon skeleton.
[0013] Optionally, the heating temperature of the calcination and carbonization is 600°C-800°C, and the heating rate is 3°C / min-6°C / min.
[0014] Optionally, the step of adding the silicon-oxygen-carbon composite to molten lithium metal for a pre-lithiation reaction to obtain a silicon-carbon negative electrode material having a solid electrolyte interface film containing lithium oxide comprises: adding the silicon oxygen carbon composite to molten lithium metal; The silicon oxygen on the surface of the silicon oxygen carbon composite particles reacts with the molten lithium metal to form silicon, lithium oxide and silicate, thereby forming a solid electrolyte interface film containing lithium oxide on the surface of the silicon oxygen carbon composite particles; The silicon-oxygen-carbon composite of the solid electrolyte interface film containing lithium oxide is used as the silicon-carbon negative electrode material.
[0015] A second aspect of the present application provides a silicon-carbon negative electrode material prepared according to the above method.
[0016] A third aspect of the present application provides a lithium battery comprising a silicon-carbon negative electrode material.
[0017] The technical solution provided by this application may have the following beneficial effects: In an embodiment of the present application, a first solution and a second solution are prepared in advance, the first solution and the second solution are mixed evenly to obtain a silicon-carbon mixed solution, a sacrificial template is added to the silicon-carbon mixed solution and mixed evenly to obtain a precursor solution, and the precursor solution is freeze-dried to obtain a precursor, the precursor is calcined and carbonized and sampled to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton, the silicon-oxygen-carbon composite is added to molten lithium metal for a pre-lithiation reaction, and a silicon-carbon negative electrode material containing a solid electrolyte interface film containing lithium oxide is obtained.
[0018] Compared with the related art, the technical solution of the present application, on the one hand, in the process of preparing the precursor, combines silicon and carbon together to form a silicon-carbon mixed liquid to solve the problem of silicon agglomeration, and freeze-drys, calcines, carbonizes and processes the sample one by one to form a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton, which is beneficial to disperse stress during charging and discharging and alleviate the volume effect. On the other hand, the silicon-oxygen-carbon composite can be subjected to a pre-lithiation reaction with molten lithium metal to obtain a silicon-carbon negative electrode material containing a solid electrolyte interface film of lithium oxide, thereby alleviating the volume effect while reducing interface side reactions, thereby improving the overall performance and safety of lithium batteries.
[0019] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The above and other objects, features and advantages of the present application will become more apparent by describing in more detail the exemplary embodiments of the present application in conjunction with the accompanying drawings, wherein the same reference numerals generally represent the same components in the exemplary embodiments of the present application.
[0021] Figure 1 It is a schematic flow chart of a method for preparing a silicon-carbon negative electrode material shown in an embodiment of the present application; Figure 2 is another schematic flow chart of a method for preparing a silicon-carbon negative electrode material shown in an embodiment of the present application; Figure 3 Schematic diagram of voltage-specific capacity curves of Examples 1-5 and Comparative Example 1 in the first week shown in the embodiments of the present application; Figure 4 It is a schematic diagram of the capacity retention rate of Examples 1-5 and Comparative Example 1 shown in the embodiments of the present application after 100 cycles of charge and discharge under 0.5C / 0.5C conditions. DETAILED DESCRIPTION
[0022] The embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and to fully convey the scope of the present application to those skilled in the art.
[0023] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0024] It should be understood that although the terms "first", "second", "third", etc. may be used in this application to describe various information, this information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of this application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0025] The volume effect refers to the volume change of the material due to the insertion and extraction of lithium ions during the electrochemical process. This volume change has a significant impact on the material structure and battery performance, and is particularly evident in high-capacity electrode materials such as silicon.
[0026] From the perspective of actual usage, silicon reacts with lithium during charging to form a lithiated silicon alloy, whose volume expands by more than 300%. During discharge, lithium is released from silicon and the volume shrinks significantly again. The drastic volume changes brought about by the charging and discharging process of the silicon negative electrode material can easily lead to mechanical stress concentration in the material, which in turn causes particle breakage and pulverization, causing lithium batteries using silicon negative electrode materials to experience problems such as conductive network breakage, electrode material failure, and short battery life.
[0027] Interfacial side reactions refer to unexpected chemical reactions between electrode materials and electrolytes or inside electrode materials in electrochemical systems. In silicon anode materials, especially when materials with large specific surface areas are used, interfacial side reactions are particularly prominent, which are mainly reflected in the following aspects: Electrolyte decomposition: During the charge and discharge process, the solutes in the electrolyte may decompose to produce gas or solid precipitates. These products will react with the electrode materials and affect the stability and cycle life of the battery.
[0028] Changes in the composition of the solid electrolyte interface membrane: Interface side reactions may change the composition and properties of the solid electrolyte interface membrane, causing it to lose its original protective function, resulting in a decrease in battery performance or reduced safety.
[0029] Reduced battery cycle stability: The presence of interfacial side reactions will accelerate the battery capacity decay, increase internal resistance and the decline of electrochemical performance, resulting in a short battery life.
[0030] Therefore, although silicon negative electrode materials with large specific surface area can effectively alleviate the volume effect of silicon, it is also necessary to deal with interfacial side reactions at the same time to ensure the overall performance and safety of the battery.
[0031] In view of the above problems, an embodiment of the present application provides a method for preparing a silicon-carbon negative electrode material, which can reduce the interfacial side reactions while effectively alleviating the volume effect, thereby improving the overall performance and safety of the battery.
[0032] The technical solution of the embodiments of the present application is described in detail below with reference to the accompanying drawings.
[0033] Figure 1 Schematic diagram of a method for preparing a silicon-carbon negative electrode material shown in an embodiment of the present application. Figure 1 , the method comprises at least the following steps.
[0034] Step 101: prepare a first solution and a second solution in advance.
[0035] In the embodiment of the present application, the first solution and the second solution may be prepared in advance.
[0036] Optionally, the first solution may be a solution containing silicon, and the second solution may be a solution containing carbon.
[0037] Step 102, mixing the first solution and the second solution evenly to obtain a silicon-carbon mixed solution.
[0038] In the embodiment of the present application, the first solution and the second solution are mixed evenly in a set manner to obtain a silicon-carbon mixed solution.
[0039] Optionally, the setting method includes adding the second solution dropwise into the first solution using a rubber-tipped dropper.
[0040] Step 103, adding the sacrificial template into the silicon-carbon mixed solution and mixing them evenly to obtain a precursor solution, and freeze-drying the precursor solution to obtain a precursor.
[0041] In an embodiment of the present application, a precursor solution is obtained by adding a sacrificial template to a silicon-carbon mixed solution and mixing the mixture evenly, and then the precursor solution is freeze-dried so that the water in the precursor solution is completely sublimated to obtain a precursor.
[0042] Alternatively, sacrificial template refers to a temporary structure or material used during manufacturing or material processing with the intention of being removed after the main manufacturing steps are completed to create complex shapes or holes and form the desired final structure.
[0043] In the present application, the sacrificial template is mainly used to form a three-dimensional porous structure to ensure that the obtained silicon-carbon negative electrode material has a three-dimensional porous structure, thereby effectively alleviating the volume effect.
[0044] Freeze drying refers to the removal of water from materials through freezing and vacuum sublimation.
[0045] Step 104 , calcining and carbonizing the precursor and performing sample treatment to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton.
[0046] In the embodiment of the present application, after obtaining the precursor, the precursor can be subjected to calcination carbonization and sample treatment to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton.
[0047] Alternatively, calcination carbonization refers to the process of converting a precursor into a carbon material by high temperature treatment.
[0048] Sample processing refers to a series of post-processing operations performed on samples during the material preparation process in order to obtain the desired material properties and morphology. In this application, sample processing includes at least washing, filtration, drying and other processes.
[0049] Step 105 , adding the silicon-oxygen-carbon composite into molten lithium metal to perform a pre-lithiation reaction to obtain a silicon-carbon negative electrode material having a solid electrolyte interface film containing lithium oxide.
[0050] In an embodiment of the present application, a silicon-oxygen-carbon negative electrode material having a solid electrolyte interface film containing lithium oxide is obtained by adding a silicon-oxygen-carbon composite into molten lithium metal for a pre-lithiation reaction.
[0051] Optionally, the pre-lithiation reaction refers to the introduction of lithium ions into the material in advance during the preparation of the electrode material, so as to improve the first cycle efficiency of the battery and reduce the irreversible capacity loss through the pre-lithiation reaction.
[0052] Solid Electrolyte Interphase (SEI) refers to a solid film formed on the surface of the negative electrode of a lithium-ion battery, which can stabilize the interface of the battery, prevent further electrolyte dissolution and reaction between the solid electrolyte and the electrode material, thereby protecting the performance and safety of the battery.
[0053] Furthermore, the solid electrolyte interface film containing lithium oxide can form a stable chemical structure in the interface, thereby effectively preventing direct contact between the electrolyte and the electrode material, preventing unnecessary electrochemical reactions, and thereby improving the cycle stability, life and safety of the battery.
[0054] In addition, the solid electrolyte interface membrane containing lithium oxide also has good ionic conductivity, which helps lithium ions to be quickly transmitted in the interface and improves the charging and discharging efficiency of the battery.
[0055] In an embodiment of the present application, a first solution and a second solution are prepared in advance, the first solution and the second solution are mixed evenly to obtain a silicon-carbon mixed solution, a sacrificial template is added to the silicon-carbon mixed solution and mixed evenly to obtain a precursor solution, and the precursor solution is freeze-dried to obtain a precursor, the precursor is calcined and carbonized and sampled to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton, the silicon-oxygen-carbon composite is added to molten lithium metal for a pre-lithiation reaction, and a silicon-carbon negative electrode material containing a solid electrolyte interface film containing lithium oxide is obtained.
[0056] Compared with the related art, the technical solution of the present application, on the one hand, in the process of preparing the precursor, combines silicon and carbon together to form a silicon-carbon mixed liquid to solve the problem of silicon agglomeration, and freeze-drys, calcines, carbonizes and processes the sample one by one to form a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton, which is beneficial to disperse stress during charging and discharging and alleviate the volume effect. On the other hand, the silicon-oxygen-carbon composite can be subjected to a pre-lithiation reaction with molten lithium metal to obtain a silicon-carbon negative electrode material containing a solid electrolyte interface film of lithium oxide, thereby alleviating the volume effect while reducing interface side reactions, thereby improving the overall performance and safety of lithium batteries.
[0057] Figure 2 It is a schematic flow chart of a method for preparing a silicon-carbon negative electrode material shown in another embodiment of the present application. Figure 2 relatively Figure 1 The technical solution of the embodiment of the present application is described in more detail. The method may include the following steps.
[0058] Step 201, dissolving a silicon source into an aqueous ammonia solution to obtain a first solution.
[0059] In the embodiment of the present application, the aqueous ammonia solution is weakly alkaline, and using the aqueous ammonia solution as a solvent helps to fully dissolve the silicon source and form a stable mixed solution.
[0060] The silicon source is silicon oxide, and the silicon oxide may specifically be one of silicon monoxide and silicon dioxide.
[0061] As an example, silicon oxide may be slowly added to a solution containing aqueous ammonia while being stirred, and stirring may be continued for a period of time to ensure that the silicon source is fully dissolved.
[0062] In addition, by controlling the amount of silicon source added, the Si content in the subsequently generated three-dimensional porous carbon framework can be flexibly adjusted.
[0063] Step 202, dissolving a carbon source in deionized water to obtain a second solution.
[0064] In the embodiment of the present application, deionized water is used as a solvent, and the carbon source is dissolved in the deionized water, so that the carbon source is fully dissolved and a uniform mixed solution is formed.
[0065] Wherein, the carbon source is one of glucose, polyacrylonitrile and polyvinyl pyrrolidone.
[0066] As an example, glucose can be slowly added to deionized water while stirring, and stirring is continued for a period of time to ensure that the carbon source is completely dissolved.
[0067] Step 203, adding the second solution dropwise into the first solution, and mixing evenly to obtain a silicon-carbon mixed solution; specifically, a rubber-tipped dropper can be used to add the second solution dropwise into the first solution.
[0068] In the embodiment of the present application, the second solution is added dropwise into the first solution, so that the carbon source in the second solution and the silicon source in the first solution can be evenly mixed to obtain a silicon-carbon mixed solution.
[0069] Step 204, adding sodium chloride to the silicon-carbon mixed solution and mixing them evenly to obtain a precursor solution.
[0070] In the embodiment of the present application, NaCl is selected as a sacrificial template, and sodium chloride is added to a mixed solution containing a silicon source and a carbon source, and the mixture is mixed evenly to obtain a precursor solution.
[0071] Step 205, transfer the precursor solution to a freeze dryer, heat the precursor solution from the starting temperature to room temperature according to a preset temperature increase gradient and temperature increase rate, and maintain each temperature stage for a period of time until the water content of the precursor solution is completely sublimated to obtain a precursor.
[0072] In the embodiment of the present application, the starting temperature is -50°C, the temperature rising gradient is 10°C, the temperature rising rate is 8°C / min-12°C / min, and the holding time of each temperature stage is 2 hours to 6 hours.
[0073] Due to the presence of a sacrificial template (NaCl) in the precursor solution, during the freeze-drying process, NaCl can spontaneously assemble into a three-dimensional porous structure when it recrystallizes. At the same time, its surface can be evenly covered with silicon sources and carbon sources, thereby combining silicon and carbon together to form a composite material, avoiding the problem of silicon easily agglomerating in its pure form.
[0074] As an example, the prepared precursor solution is transferred to a freeze dryer, and the starting temperature of the freeze dryer is set to -50°C to ensure that the precursor solution is quickly frozen into solid ice, the heating rate is set to 10°C / min, and the holding time of each temperature stage is set to 4 hours. One minute later, the precursor solution reaches -40°C, and the temperature is maintained for 4 hours to ensure that the water in this section is completely sublimated. The temperature is continued to be increased at a gradient of 10°C, and the precursor solution is increased from -40°C to -30°C. The temperature is maintained for 4 hours to ensure that the water in this section is completely sublimated. The temperature is continuously heated according to the set heating rate and heating gradient until the temperature of the precursor solution reaches room temperature. At this time, the water in the precursor solution is completely sublimated to obtain a water-free precursor.
[0075] Step 206, calcining and carbonizing the precursor under a protective atmosphere; specifically, transferring the precursor to a tubular furnace filled with a protective atmosphere for calcining and carbonizing.
[0076] In the embodiments of the present application, the precursor is calcined and carbonized under a protective atmosphere to convert the silicon source into silicon oxide and the carbon source into carbon, thereby effectively extracting silicon oxide and carbon material, providing a basis for preparing a composite material.
[0077] Protective atmosphere refers to an inert gas or specific gas environment used during material processing or reaction to prevent the material from reacting adversely with oxygen or other active gases in the air.
[0078] In the present application, the protective atmosphere may be argon or other inert gases.
[0079] In the present application, the heating temperature of calcination and carbonization is 600° C.-800° C., and the heating rate is 3° C. / min-6° C. / min.
[0080] As an example, the interior of the tube furnace is first evacuated, and then argon gas is introduced, and the heating temperature for calcination and carbonization is set to 600°C, and the heating rate is set to 3°C / min. Then, the freeze-dried precursor is placed in the tube furnace and calcined for 5 hours to ensure that the precursor is fully carbonized. During the carbonization process, the silicon source is converted into silicon oxide (SiO x ), the carbon source is converted into carbon, and both are coated on the surface of NaCl, NH4 + Escapes as gas.
[0081] Step 207, washing the calcined and carbonized precursor with deionized water, filtering and drying to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton.
[0082] In the embodiment of the present application, the precursor is first washed with deionized water to remove the NaCl template and byproducts generated during the calcination and carbonization process, thereby ensuring the purity of the precursor. The solution and solid precursor generated during the washing process are then separated by suction filtration, and then the water in the precursor is removed by drying to obtain a high-purity silicon-oxygen-carbon composite (in the present application, the silicon-oxygen-carbon composite is represented by SiOx@C).
[0083] Among them, the silicon-oxygen-carbon composite refers to a composite in which silicon oxide is wrapped by carbon material or embedded in a three-dimensional porous carbon skeleton.
[0084] As an example, the NaCl template is removed by washing, filtration and drying to obtain SiO x SiO coated on a three-dimensional porous carbon framework x @C.
[0085] Step 208 , adding the silicon-oxygen-carbon composite into molten lithium metal to perform a pre-lithiation reaction to obtain a silicon-carbon negative electrode material having a solid electrolyte interface film containing lithium oxide.
[0086] In the present embodiment, lithium foil is placed in a stainless steel shell, heated to melt at a temperature range of 250-330°C, and then a slightly excessive amount of SiO is added. x @C makes it react. Because metallic lithium has a strong reducing property, it can spontaneously react with SiO x @C (its three-dimensional porous carbon skeleton is covered with SiO x ) surface silicon oxide (SiO x ) reacts, decomposes and converts into Si, Li2O and silicate, forms a solid electrolyte interface film containing lithium oxide on the surface of the silicon-oxygen-carbon composite particles, and the silicon-oxygen-carbon composite with the solid electrolyte interface film containing lithium oxide is used as the silicon-carbon negative electrode material.
[0087] As an example, under high temperature conditions, such as 250°C-330°C, lithium metal is melted, and the molten Li undergoes a redox reaction with the oxide, thereby converting SiO x Reduction is performed to obtain Si, Li2O and silicate, thereby forming a solid electrolyte interface film rich in lithium oxide on the surface of the silicon-oxygen-carbon composite particles.
[0088] The present application uses NaCl as a sacrificial template and adopts freeze drying, high temperature carbonization, washing, filtration, drying and pre-lithiation to prepare a solid electrolyte membrane (SEI) rich in lithium oxide (Li2O) formed on the surface of silicon-oxygen-carbon composite particles, thereby obtaining a silicon-carbon negative electrode material with a three-dimensional porous carbon skeleton and a solid electrolyte membrane rich in lithium oxide, thereby achieving the reduction of interfacial side reactions while effectively alleviating the volume effect, thereby improving the overall performance and safety of lithium batteries.
[0089] The following describes in detail the technical solution and testing process of the present application through multiple embodiments: Example 1-3: Add a certain mass of SiO2 (1g of SiO2 in Example 1, 1.3g of SiO2 in Example 2, and 1.5g of SiO2 in Example 3) and 10ml of NH3·H2O to 500ml of ethanol, stir for 20min as solution 1, add 10g of glucose to 10ml of deionized water and stir evenly as solution 2, add solution 2 dropwise to solution 1 using a rubber-tipped dropper, stir for 2h, then add 20g of NaCl, and stir the mixed solution at room temperature for 4h. Then transfer the mixed precursor solution to a vacuum freeze dryer, and heat it step by step from -50℃ to room temperature according to a temperature increase gradient of 10℃, and keep it for 4 hours in each insulation stage until all the water in the precursor solution sublimates. The freeze-dried precursor is calcined in a tube furnace (argon atmosphere) at 600℃ for 5h for carbonization, with a heating rate of 3℃ / min. Afterwards, the product was washed with deionized water and filtered to remove the auxiliary template NaCl in the product, and dried in a vacuum oven at 60 °C overnight to obtain the product SiO x @C. Finally, a slightly excess of SiO x @C (capacity calculated as 1600mAh / g) is added to 300°C molten lithium (capacity calculated as 3860mAh / g) for pre-lithiation reaction to obtain the final product, silicon-carbon negative electrode material.
[0090] Among them, different SiO2 addition amounts (1g, 1.3g, 1.5g) in the precursor solution can obtain silicon-carbon negative electrode materials with different Si contents. The silicon-carbon negative electrode materials of Examples 1-3 are named SiC-1, SiC-2 and SiC-3, respectively.
[0091] In Example 1, the process of preparing the working electrode of the lithium-ion battery using SiC-1 and performing electrochemical testing can be: SiC-1: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 and evenly coated on a 10um copper foil. They were dried in a vacuum oven at 80°C for 12 hours, and then the pole pieces were compacted and punched into pole pieces with a diameter of 12mm using a roller press. The surface density was 5-6 mg / cm 2 The electrode was used as the working electrode and lithium metal as the counter electrode, and the half-cell was assembled in a glove box. The separator was a 18um thick polypropylene (PP) separator, and the electrolyte was 1 mol / L lithium hexafluorophosphate (LiPF6) in ethylene carbonate (EC) / diethyl carbonate (DEC) solvent (volume ratio: v / v=1:1).
[0092] At room temperature, the battery was electrochemically tested using relevant battery testing equipment. The charge and discharge mode for the first week was 0.1C / 0.1C, followed by 0.5C / 0.5C for 100 weeks. The voltage range was 0.005-2V, and 1C=1600mA / g.
[0093] Example 2: The process of preparing a working electrode of a lithium-ion battery using SiC-2 and performing an electrochemical test may be: SiC-2: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 and evenly coated on a 10um copper foil. The mixture was dried in a vacuum oven at 80°C for 12 hours. The pole pieces were then compacted and punched into pole pieces with a diameter of 12mm using a roller press. The surface density was 5-6 mg / cm 2 The electrode was used as the working electrode and lithium metal as the counter electrode, and the half-cell was assembled in a glove box. The separator was a 18um thick polypropylene (PP) separator, and the electrolyte was 1 mol / L LiPF6 in EC / DEC (v / v=1:1) solvent.
[0094] At room temperature, the battery was electrochemically tested using relevant battery testing equipment. The charge and discharge mode for the first week was 0.1C / 0.1C, followed by 0.5C / 0.5C for 100 weeks. The voltage range was 0.005-2V, and 1C=1600mA / g.
[0095] Example 3: The process of preparing a working electrode of a lithium-ion battery using SiC-3 and performing an electrochemical test may be: SiC-3: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 and evenly coated on a 10um copper foil. The mixture was dried in a vacuum oven at 80°C for 12 hours. The pole pieces were then compacted and punched into pole pieces with a diameter of 12mm using a roller press. The surface density was 5-6 mg / cm 2 The electrode was used as the working electrode and lithium metal as the counter electrode, and the half-cell was assembled in a glove box. The separator was a 18um thick polypropylene (PP) separator, and the electrolyte was 1 mol / L LiPF6 in EC / DEC (v / v=1:1) solvent.
[0096] At room temperature, the battery was electrochemically tested using relevant battery testing equipment. The charge and discharge mode for the first week was 0.1C / 0.1C, followed by 0.5C / 0.5C for 100 weeks. The voltage range was 0.005-2V, and 1C=1600mA / g.
[0097] Example 4: Add 0.73g of SiO and 10ml of NH3·H2O to 500ml of ethanol, stir for 20min as solution 1, add 17g of polyacrylonitrile to 10ml of deionized water and stir evenly as solution 2, add solution 2 dropwise to solution 1 using a rubber-tipped dropper, stir for 2h, add 20g of NaCl, and stir the mixed solution at room temperature for 4h. Then transfer the mixed precursor solution to a vacuum freeze dryer, and heat it step by step from -50℃ to room temperature according to a temperature increase gradient of 10℃, and keep it for 6 hours in each insulation stage until all the water in the precursor solution sublimates. The freeze-dried precursor is calcined in a tube furnace at 800℃ (argon atmosphere) for 5h for carbonization, with a heating rate of 5℃min-1. Afterwards, wash with deionized water and filter to remove the auxiliary template NaCl in the product, and dry it in a vacuum oven at 60℃ overnight to obtain the product SiO x @C. Finally, a slightly excess of SiO x @C (capacity calculated as 1600mAh / g) is added to 300°C molten lithium (capacity calculated as 3860mAh / g) for pre-lithiation reaction to obtain the final product, silicon-carbon negative electrode material (SiC-4).
[0098] In Example 4, the process of preparing the working electrode of the lithium ion battery using SiC-4 and performing electrochemical testing can be: SiC-4: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 and evenly coated on a 10um copper foil. The mixture was dried in a vacuum oven at 80°C for 12 hours. The pole pieces were then compacted and punched into pole pieces with a diameter of 12mm using a roller press. The surface density was 5-6 mg / cm 2 The electrode was used as the working electrode and lithium metal as the counter electrode, and the half-cell was assembled in a glove box. The separator was a 18um thick polypropylene (PP) separator, and the electrolyte was 1 mol / L lithium hexafluorophosphate (LiPF6) in ethylene carbonate (EC) / diethyl carbonate (DEC) solvent (volume ratio: v / v=1:1).
[0099] At room temperature, the battery was electrochemically tested using relevant battery testing equipment. The charge and discharge mode for the first week was 0.1C / 0.1C, followed by 0.5C / 0.5C for 100 weeks. The voltage range was 0.005-2V, and 1C=1600mA / g.
[0100] Example 5: Add 1g of SiO2 and 10ml of NH3·H2O to 500ml of ethanol and stir for 20min as solution 1. Add 16g of polyvinyl pyrrolidone to 10ml of deionized water and stir evenly as solution 2. Use a rubber-tipped dropper to add solution 2 dropwise to solution 1. After stirring for 2h, add 20g of NaCl and stir the mixed solution at room temperature for 4h. Then transfer the mixed precursor solution to a vacuum freeze dryer and heat it step by step from -50℃ to room temperature according to a temperature increase gradient of 10℃, and keep it for 2 hours in each insulation stage until all the water in the precursor solution sublimates. The freeze-dried precursor is calcined in a tube furnace at 600℃ (argon atmosphere) for 5h for carbonization, with a heating rate of 3℃min-1. Afterwards, wash with deionized water and filter to remove the auxiliary template NaCl in the product, and dry it in a vacuum oven at 60℃ overnight to obtain the product SiO x @C. Finally, a slightly excess of SiO x @C (capacity calculated as 1600mAh / g) was added to 300°C molten lithium (capacity calculated as 3860mAh / g) for pre-lithiation reaction to obtain the final product, silicon-carbon negative electrode material (SiC-5).
[0101] In Example 5, the process of preparing the working electrode of a lithium-ion battery using SiC-5 and performing electrochemical testing may be: SiC-5: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 and evenly coated on a 10um copper foil. The mixture was dried in a vacuum oven at 80°C for 12 hours. The pole pieces were then compacted and punched into pole pieces with a diameter of 12mm using a roller press. The surface density was 5-6 mg / cm 2 The electrode was used as the working electrode and lithium metal as the counter electrode, and the half-cell was assembled in a glove box. The separator was a 18um thick polypropylene (PP) separator, and the electrolyte was 1 mol / L lithium hexafluorophosphate (LiPF6) in ethylene carbonate (EC) / diethyl carbonate (DEC) solvent (volume ratio: v / v=1:1).
[0102] At room temperature, the battery was electrochemically tested using relevant battery testing equipment. The charge and discharge mode for the first week was 0.1C / 0.1C, followed by 0.5C / 0.5C for 100 weeks. The voltage range was 0.005-2V, and 1C=1600mA / g.
[0103] Comparative Example 1: Graphite: carbon black: carboxymethyl cellulose lithium (CMC): polystyrene butadiene (SBR) were mixed in a ratio of 80:10:5:5 and evenly coated on a 10um copper foil, dried in a vacuum oven at 80°C for 12h, and then the pole piece was compacted and punched into a pole piece with a diameter of 12mm using a roller press, with a surface density of 5-6 mg / cm 2 The electrode was used as the working electrode and lithium metal as the counter electrode, and the half-cell was assembled in a glove box. The separator was a 18um thick polypropylene (PP) separator, and the electrolyte was 1 mol / L LiPF6 in EC / DEC (v / v=1:1) solvent.
[0104] At room temperature, the battery was electrochemically tested using relevant battery testing equipment. The charge and discharge mode for the first week was 0.1C / 0.1C, followed by 0.5C / 0.5C for 100 weeks. The voltage range was 0.005-2V, and 1C=360mA / g.
[0105] Referring to the following Table 1, Table 1 shows various test performance parameters of the lithium ion batteries prepared in Examples 1-5 and Comparative Example 1.
[0106]
[0107] Table 1 Based on the actual test voltage, specific capacity and various test performance parameters in Table 1 above, the Figure 3 and Figure 4 . Figure 3 This is a schematic diagram of the voltage-specific capacity curves of Examples 1-5 and Comparative Example 1 in the first week shown in the embodiments of the present application, Figure 3 The ordinate represents the charge and discharge voltage, and the abscissa represents the specific capacity, which can reflect the battery capacity, stability and other aspects of each embodiment and comparative example. Figure 4 This is a schematic diagram of the capacity retention rate of Examples 1-5 and Comparative Example 1 shown in the embodiments of the present application under 0.5C / 0.5C conditions for 100 cycles of charge and discharge, Figure 4 The ordinate represents the capacity retention rate, and the abscissa represents the number of cycles, which can reflect the capacity retention of each embodiment and comparative example after multiple charge and discharge cycles.
[0108] From Table 1, Figure 3 as well as Figure 4 It can be seen that there are certain differences in the first week charging capacity, initial charge and discharge efficiency, and capacity retention rate after 100 cycles of silicon-carbon negative electrode materials with different Si contents.
[0109] Compared with Comparative Example 1, Examples 1, 2, 3, 4, and 5 can not only meet the requirements of high energy density, but also effectively alleviate the volume effect. At the same time, they can effectively isolate the direct contact between the silicon negative electrode and the electrolyte by forming a solid electrolyte interface film rich in lithium oxide, thereby reducing the occurrence of interfacial side reactions.
[0110] The charging capacity of Examples 1, 2, 3, 4, and 5 is relatively high, which means that the lithium-ion battery has a relatively high charge storage capacity during a single charge. The first efficiency of Examples 1, 2, 3, 4, and 5 can be maintained at a relatively high level, ensuring that the energy conversion rate of the lithium-ion battery is high during the first charge and discharge process.
[0111] Among them, after 100 cycles, the capacity retention rates of Examples 1, 2, and 4 are at a relatively high level, and Examples 1, 2, and 4 have high stability and performance, which are conducive to long-term cyclic use. In particular, Example 1 still has a capacity retention rate of 94.74% after 100 cycles at room temperature 0.5°C.
[0112] In actual use, different embodiments can be selected to prepare lithium-ion batteries according to specific application requirements. For example, if long-term use and cyclic charge and discharge are required, embodiment 1 can be selected. If high charging capacity and certain long-term stability are required, embodiment 2, embodiment 3 or embodiment 5 can be selected. If comprehensive performance such as high charging capacity, good initial efficiency and long-term use are required, embodiment 4 can be selected.
[0113] It should be noted that the embodiments of the present application include but are not limited to the above examples. It is understandable that under the guidance of the ideas of the embodiments of the present application, technical personnel in this field can make settings according to actual conditions, and the present application does not limit this.
[0114] In order to enable those skilled in the art to better understand the technical solution of the embodiment of the present application, the embodiment of the present application is explained below by using an example.
[0115] a) dissolving a silicon source in a solution to which aqueous ammonia is added to obtain solution 1; b) dissolving a carbon source in deionized water to obtain a second solution; c) Use a rubber-tipped dropper to add solution 2 dropwise into solution 1 and mix well; d) adding NaCl as a sacrificial template to a mixed solution containing a silicon source and a carbon source, and mixing them evenly to obtain a precursor solution; e) transferring the precursor solution to a freeze dryer for freeze drying to completely sublime the water; f) placing the precursor obtained in step e into a tube furnace filled with argon gas for calcination and carbonization, and then washing with deionized water, filtering, and drying to obtain a silicon-oxygen-carbon composite (SiO x@C); g) The SiO obtained in step f is x @C is added to molten lithium metal for pre-lithiation reaction to obtain the final product, silicon-carbon negative electrode material.
[0116] In step a), the silicon source is one of SiO and SiO2, and the role of ammonia water is to make the solution weakly alkaline, which is conducive to the dissolution of the silicon source.
[0117] In step b), the carbon source is one of glucose, polyacrylonitrile and polyvinyl pyrrolidone.
[0118] In step c), the purpose of adding dropwise is to uniformly mix the carbon source and the silicon source.
[0119] In step e), the temperature is gradually increased from -50°C to room temperature at a rate of 8-12°C / min, and each insulation stage is maintained for 2-6 hours.
[0120] In step f), the heating temperature is 600-800° C., and the heating rate is 3-6° C. / min.
[0121] In step g), the lithium foil is placed in a stainless steel shell, heated to melt at a temperature range of 250-330°C, and then a slightly excess amount of SiO x @C makes it react. Because metallic lithium has a strong reducing property, it can spontaneously react with SiO x @C reacts and converts into Si, Li2O and silicate.
[0122] According to the above method, a silicon-carbon negative electrode material with a three-dimensional porous structure and a stable interface is prepared.
[0123] In the present embodiment, the silicon source, carbon source and NaCl are first mixed into a uniform solution. During the freeze-drying process, NaCl recrystallizes and spontaneously assembles into a three-dimensional porous structure, and its surface can be evenly covered with the silicon source and carbon source. In the subsequent calcination process, the silicon source is converted into SiO x , the carbon source is converted into carbon, and both are coated on the surface of NaCl, while NH4 + Then, the NaCl template was removed by water washing and filtration to obtain SiO x SiO coated on a three-dimensional porous carbon framework x @C, finally through SiO x The pre-lithiation reaction between the silicon and molten lithium produces a silicon-carbon composite material rich in Li2O film.
[0124] After the above preparation steps, the present application can at least obtain the following beneficial effects: 1. In the process of preparing the precursor, the compound between silicon and carbon can improve the agglomeration problem of silicon.
[0125] 2. The three-dimensional porous carbon skeleton can not only maintain a stable structure and alleviate the volume effect, but also enhance conductivity. At the same time, the Li2O-rich SEI film formed during the pre-lithiation process has a more stable structure, higher interface energy and lithium ion transmission speed than ordinary SEI, which can enhance the interface stability of silicon.
[0126] 3. In addition, by controlling the amount of SiO2 added in the precursor and adjusting the Si content in the three-dimensional porous carbon skeleton, silicon-carbon negative electrode materials with different capacities can be obtained. The lithium battery prepared using the silicon-carbon negative electrode material as the working electrode can exhibit excellent electrochemical properties.
[0127] In addition, an embodiment of the present application further provides a silicon-carbon negative electrode material, which is prepared according to the above-mentioned preparation method.
[0128] An embodiment of the present application further provides a lithium battery, which includes the above-mentioned silicon-carbon negative electrode material.
[0129] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A method for preparing a silicon-carbon negative electrode material, characterized in that: include: Pre-preparing a first solution and a second solution; Evenly mixing the first solution and the second solution to obtain a silicon-carbon mixed solution; Adding a sacrificial template to the silicon-carbon mixed solution and mixing them evenly to obtain a precursor solution, and freeze-drying the precursor solution to obtain a precursor; The precursor is subjected to calcination and carbonization and sample treatment to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton; The silicon-oxygen-carbon composite is added into molten lithium metal to carry out a pre-lithiation reaction, thereby obtaining a silicon-carbon negative electrode material containing a solid electrolyte interface film of lithium oxide.
2. The method according to claim 1, characterized in that The pre-prepared first solution and second solution include: dissolving a silicon source into an aqueous ammonia solution to obtain the first solution; dissolving a carbon source in deionized water to obtain the second solution; Wherein, the silicon source is one of silicon monoxide and silicon dioxide, and the carbon source is one of glucose, polyacrylonitrile and polyvinyl pyrrolidone.
3. The method according to claim 1, characterized in that The first solution and the second solution are mixed evenly to obtain a silicon-carbon mixed solution, comprising: The second solution is added dropwise into the first solution, and after mixing evenly, the silicon-carbon mixed solution is obtained.
4. The method according to claim 1, characterized in that: The sacrificial template is sodium chloride, and the sacrificial template is added to the silicon-carbon mixed solution and mixed evenly to obtain a precursor solution, comprising: Adding the sodium chloride into the silicon-carbon mixed solution and mixing them evenly to obtain the precursor solution; The freeze-drying of the precursor solution to obtain the precursor comprises: The precursor solution is transferred to a freeze dryer, and the precursor solution is heated from the starting temperature to room temperature according to a preset temperature increase gradient and temperature increase rate, and maintained at each temperature stage for a period of time until the water content of the precursor solution is completely sublimated to obtain the precursor.
5. The method according to claim 4, characterized in that The starting temperature is -50°C, the temperature rising gradient is 10°C, the temperature rising rate is 8°C / min-12°C / min, and the holding time of each temperature stage is 2h-6h.
6. The method according to claim 2, characterized in that The sample treatment includes washing, filtering and drying, and the precursor is subjected to calcination, carbonization and sample treatment to obtain a silicon-oxygen-carbon composite in which silicon and oxygen are covered on a three-dimensional porous carbon skeleton, including: The precursor is calcined and carbonized under a protective atmosphere to convert the silicon source into silicon oxide and the carbon source into carbon; the carbon and the silicon oxide are coated on the surface of the sacrificial template; The calcined and carbonized precursor is washed, filtered and dried with deionized water to remove the sacrificial template, thereby obtaining a silicon-oxygen-carbon composite in which silicon and oxygen are covered on the three-dimensional porous carbon skeleton.
7. The method according to claim 6, characterized in that The heating temperature of the calcination and carbonization is 600° C.-800° C., and the heating rate is 3° C. / min-6° C. / min.
8. The method according to claim 1, characterized in that: The step of adding the silicon-oxygen-carbon composite to molten lithium metal for a pre-lithiation reaction to obtain a silicon-carbon negative electrode material having a solid electrolyte interface film containing lithium oxide comprises: adding the silicon oxygen carbon composite to molten lithium metal; The silicon oxygen on the surface of the silicon oxygen carbon composite particles reacts with the molten lithium metal to form silicon, lithium oxide and silicate, thereby forming a solid electrolyte interface film containing lithium oxide on the surface of the silicon oxygen carbon composite particles; The silicon-oxygen-carbon composite of the solid electrolyte interface film containing lithium oxide is used as the silicon-carbon negative electrode material.
9. A silicon-carbon negative electrode material, characterized in that: Prepared according to the method according to any one of claims 1 to 8.
10. A lithium battery, characterized in that: Contains the silicon-carbon negative electrode material according to claim 9.
Citation Information
Cited By
Three-dimensional mesoporous carbon composite silicon carbon negative electrode material and preparation method and application thereof
CN119650652A
Three-dimensional mesoporous carbon composite silicon-carbon negative electrode material and preparation method and application thereof