Magnetic metal composite material aerogel as well as preparation method and application thereof

Through hydrothermal reaction and carbonization treatment combined with MXene material, magnetic metal composite aerogel was prepared, which solved the problems of low efficiency and poor stability of existing electromagnetic materials in the field of high-frequency electromagnetic waves and low temperature environments, and achieved high-performance electromagnetic shielding Effect, suitable for electromagnetic radiation protection of modern electronic equipment.

CN119012671AActive Publication Date: 2024-11-22TONGJI UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411184547.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing electromagnetic materials have high dielectric constant and magnetic permeability in the field of high-frequency electromagnetic waves, resulting in low electromagnetic reflection and absorption efficiency, and poor stability in high-temperature environments, making it difficult to meet the high performance and reliability needs of modern electronic equipment.

Method used

Cobalt metal organic frame is synthesized through hydrothermal reaction, and through the combination of carbonization and MXene materials, a magnetic metal composite aerogel is prepared to achieve the organic combination of magnetic metal, graphene and MXene materials, and coordinate the regulation of magnetic loss and dielectricity Loss and conductivity loss improve electromagnetic shielding performance.

Benefits of technology

The prepared magnetic metal composite aerogel has excellent electromagnetic shielding performance and is suitable for the protection of electromagnetic radiation and electromagnetic pollution. It has a simple process, green and environmentally friendly, and has controllable parameters, which is suitable for applications in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119012671A_ABST
    Figure CN119012671A_ABST
Patent Text Reader

Abstract

The invention provides a magnetic metal composite material aerogel as well as a preparation method and application thereof, and relates to a multi-component composite material in the field of electromagnetic functional materials. A cobalt-based metal-organic framework (Co-MOFs) is synthesized by utilizing a hydrothermal method, the Co / C / MXene composite material aerogel with different properties is finally obtained by accurately controlling a heat treatment process of the Co-MOFs, such as carbonization temperature, atmosphere and time, and the prepared aerogel composite material realizes organic combination of magnetic metal, graphene and an MXene material, so that the magnetic metal / graphene / MXene composite material can be used for preparing a magnetic material. The electromagnetic shielding material plays a synergistic effect of magnetic loss, dielectric loss and conductive loss, has excellent electromagnetic shielding performance, and has important practical significance in the fields of electromagnetic radiation coping, electromagnetic pollution protection and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a multi-component composite material in the field of electromagnetic functional materials, and in particular to a magnetic metal composite aerogel and a preparation method and application thereof. Background Art

[0002] The development of electromagnetic materials plays a vital role in today's society, forming the foundation of modern electronics, communications, and energy. From mobile phones and computers to various communication devices, all rely on the performance of electromagnetic materials; properties such as conductivity, dielectric constant, and magnetic properties directly determine the performance and functionality of these devices. With global energy challenges becoming increasingly prominent, energy conservation and emission reduction have become crucial tasks for governments and businesses worldwide. The development of low-power, high-efficiency electromagnetic materials can reduce the energy consumption of electronic devices, extend battery life, and reduce energy consumption, thereby alleviating environmental pressure and achieving sustainable development. Furthermore, the development of electromagnetic materials is crucial for enhancing a country's scientific and technological strength and national defense capabilities. Modern military equipment has a huge demand for electromagnetic materials, and everything from radar systems to communications equipment requires high-performance and reliable electromagnetic materials. The development of electromagnetic materials is not only crucial for promoting the development of the electronics, communications, and energy industries, but also for energy conservation and emission reduction, ensuring national security, and promoting scientific and technological innovation. Therefore, increasing investment in the research and development of electromagnetic materials and promoting the advancement of their technological capabilities are crucial for promoting social progress and sustainable development.

[0003] Aerogel materials offer unique advantages in the field of electromagnetic materials. They feature extremely low density and a highly open pore structure. A porosity of over 90% enables aerogel materials to exhibit extremely low dielectric constants and permeabilities during electromagnetic wave propagation. These properties enable aerogel materials to perform exceptionally well in high-frequency electromagnetic fields, such as microwaves and radio frequency, effectively reducing reflection and absorption of electromagnetic waves and improving transmission efficiency. Aerogel materials also possess excellent thermal and chemical stability. This allows aerogel materials to maintain excellent electromagnetic properties in harsh environments, such as high temperatures and in the presence of acids and alkalis, and is not susceptible to degradation or damage. This stability holds great potential for application in high-temperature environments, such as aerospace and automotive electronics. Aerogel materials also offer excellent controllability and customization. By adjusting parameters such as aerogel composition, pore structure, and morphology, their electromagnetic properties can be precisely controlled to meet the requirements of diverse application scenarios. This controllability holds broad application prospects for aerogel materials in areas such as electromagnetic wave shielding, microwave absorption, and antenna design. Aerogel materials also offer advantages such as lightweight, environmental friendliness, and ease of processing. Due to their low density and high porosity, aerogel materials are extremely lightweight, reducing the overall weight of electronic devices and improving their portability and mobility. Furthermore, aerogel materials, typically based on inorganic aerogels, exhibit excellent weather resistance and environmental adaptability, making them less susceptible to moisture, aging, or corrosion, thus improving the lifespan and reliability of devices.

[0004] MXene is a type of two-dimensional material, typically composed of transition metal carbides. Its structural basis is hexagonal layers formed by transition metals and carbon or nitrogen. Due to this unique structure, MXene materials possess excellent electromagnetic and mechanical properties, along with a high specific surface area activity and exceptional plasticity and flexibility. Consequently, they are widely used in the manufacture of conductive inks, flexible electrodes, and transparent conductive films. Summary of the Invention

[0005] The present invention is based on the above background technology and aims to provide a magnetic metal composite aerogel and a preparation method and application thereof.

[0006] The present invention provides a method for preparing a magnetic metal composite aerogel, which has the following characteristics and comprises the following steps: S10, dissolving a cobalt salt and 2,5-dihydroxyterephthalic acid in a solvent and performing a hydrothermal reaction to obtain a cobalt metal organic framework; S20, carbonizing the cobalt metal organic framework to obtain a Co / C aerogel; S30, immersing the Co / C aerogel in a MXene solution to obtain the magnetic metal composite aerogel.

[0007] The method for preparing the magnetic metal composite aerogel provided by the present invention may also have the following characteristics: wherein, in step S10, the cobalt salt includes cobalt acetate tetrahydrate and / or cobalt chloride tetrahydrate, and the solvent includes any one or more of anhydrous ethanol, methanol or deionized water.

[0008] The method for preparing the magnetic metal composite aerogel provided by the present invention may also have the following characteristics: wherein, step S10 includes the following sub-steps: S11, mixing a cobalt salt solution and a 2,5-dihydroxyterephthalic acid solution and stirring to obtain a reaction liquid; S12, adding water to the reaction liquid and conducting a hydrothermal reaction to prepare a cobalt metal organic framework solution.

[0009] The preparation method of the magnetic metal composite aerogel provided by the present invention may also have the following characteristics: wherein, in step S11, the cobalt salt concentration in the cobalt salt solution is 20 to 40 mg / mL, the 2,5-dihydroxyterephthalic acid concentration in the 2,5-dihydroxyterephthalic acid solution is 2 to 10 mg / mL, the volume ratio of the cobalt salt solution to the 2,5-dihydroxyterephthalic acid solution is (1 to 8): (1 to 4), and the stirring time is 2 hours. In step S12, the volume ratio of the amount of water added to the reaction liquid is (1 to 3): (1 to 9), and the hydrothermal reaction conditions are: heating to 50°C to 180°C at a heating rate of 1°C / min to 10°C / min and then keeping warm for 12 hours to 24 hours.

[0010] The method for preparing the magnetic metal composite aerogel provided by the present invention may also have the following characteristics: wherein, step S20 includes the following sub-steps: S21, mixing the cobalt metal organic framework and graphene in a solvent to prepare a Co / C composite material solution; S22, freeze-drying the Co / C composite material solution and heating it under an inert atmosphere to obtain the Co / C aerogel.

[0011] The preparation method of the magnetic metal composite aerogel provided by the present invention may also have the following characteristics: wherein the mass of the cobalt metal organic framework in step S21 is recorded as m1, the mass of the graphene is recorded as m2, m1:m2=1:(4-10), and in step S22, the inert atmosphere is argon, and the heating method is: heating to 500°C to 900°C at a heating rate of 2°C / min to 10°C / min and then keeping warm for 60min to 180min.

[0012] The method for preparing the magnetic metal composite aerogel provided by the present invention may also have the following feature: in step S21, chitosan solution and ethanol are also added.

[0013] The preparation method of the magnetic metal composite aerogel provided by the present invention may also have the following characteristics: wherein, the immersion method in step S30 is: uniformly adding the MXene solution dropwise to the surface of the Co / C aerogel until the MXene solution precipitates from the bottom of the Co / C aerogel, and the Co / C aerogel is converted into a Co / C / MXene composite aerogel, that is, a magnetic metal composite aerogel, and the mass of MXene in the MXene solution in step S30 is recorded as m3, m1:m3=1:(0.01~0.2).

[0014] The present invention also provides a magnetic metal composite aerogel having the following characteristics, which is prepared by any of the aforementioned methods for preparing the magnetic metal composite aerogel.

[0015] The present invention also provides an application of a magnetic metal composite material aerogel in electromagnetic shielding, which has the following characteristics: the electromagnetic shielding performance of the magnetic metal composite material aerogel is 20-50 dB.

[0016] Functions and effects of the invention

[0017] The present invention utilizes a hydrothermal method to synthesize cobalt-based metal-organic frameworks (Co-MOFs). By precisely controlling the heat treatment process of Co-MOFs, such as the carbonization temperature, atmosphere, and time, Co / C / MXene composite aerogels with different properties are ultimately obtained. The prepared aerogel composite material realizes the organic combination of magnetic metal, graphene, and MXene materials, exerts the synergistic effect of magnetic loss, dielectric loss, and conductivity loss, and has excellent electromagnetic shielding performance, which has important practical significance in the fields of electromagnetic radiation and electromagnetic pollution protection.

[0018] This invention leverages the porous and lightweight properties of aerogel materials, combined with the excellent electromagnetic properties of MXene materials, to produce a composite aerogel with certain mechanical properties, combined with lightweight, high strength, and stable properties. This material has broad potential for development in the face of enormous market demand.

[0019] The preparation method of the magnetic metal composite aerogel of the present invention is simple, green, environmentally friendly and has controllable parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flowchart of a method for preparing a magnetic metal composite aerogel according to an embodiment of the present invention;

[0021] Figure 2 1 is the XRD pattern of sample 1, sample 2, sample 3 and the comparative sample in the test example of the present invention;

[0022] Figure 31 is the SEM image of sample 1, sample 2, sample 3 and the comparative sample in the test example of the present invention;

[0023] Figure 4 EMI performance curves of sample 1, sample 2, sample 3 and the comparative sample in the test example of the present invention. DETAILED DESCRIPTION

[0024] In order to make the technical means, creative features, objectives and effects of the present invention easier to understand, the following examples and accompanying drawings specifically illustrate a magnetic metal composite aerogel, its preparation method and application of the present invention.

[0025] <Example>

[0026] Figure 1 It is a flowchart of a method for preparing a magnetic metal composite aerogel according to an embodiment of the present invention.

[0027] like Figure 1 As shown, this embodiment provides a method for preparing a magnetic metal composite aerogel, comprising the following steps:

[0028] S10, preparing a cobalt metal organic framework, comprising the following sub-steps:

[0029] S11, preparing 100 mL of a methanol solution of x1 g of a cobalt salt and 50 mL of a methanol solution of x2 g of 2,5-dihydroxyterephthalic acid, mixing the mixture, stirring continuously for 2 h, and allowing the mixture to react fully to obtain a reaction solution;

[0030] S12, adding 50 mL of water to the reaction solution and performing a hydrothermal reaction at 180° C. for 12 h to prepare a cobalt metal organic framework solution.

[0031] S20, carbonizing the cobalt metal organic framework to obtain a Co / C aerogel, comprising the following sub-steps:

[0032] S21, concentrating the cobalt metal organic framework solution in step S12 to a fixed volume and mixing it with the graphene solution, adding 6.25 mL of a 40 mg / mL chitosan solution to facilitate subsequent aerogel formation, and adding 1 mL of ethanol to enhance surface tension to prepare 20 mL of a Co / C composite material solution;

[0033] S22, the Co / C composite material solution was stirred for 3 h to ensure the uniformity of the solution, frozen for 12 h, freeze-dried for 24 h, and then kept warm in an Ar atmosphere at T °C for 2 h to obtain the Co / C aerogel.

[0034] S30, preparing a magnetic metal composite aerogel, comprising the following sub-steps:

[0035] S31, using HCl / LiF mixed solution to etch Ti3AlC2 to prepare MXene solution and controlling its concentration to x3 mg / mL;

[0036] S32, 5 mL of MXene solution was evenly added dropwise to the surface of the Co / C aerogel until the MXene solution precipitated from the bottom of the Co / C aerogel, and the product was then vacuum dried for 12 h. The Co / C aerogel was converted into a Co / C / MXene composite aerogel, and a magnetic metal composite aerogel was obtained.

[0037] This embodiment also provides a magnetic metal composite aerogel, which is prepared by the preparation method of the magnetic metal composite aerogel provided in this embodiment.

[0038] In this example, by regulating the specific parameters in the preparation process, three magnetic metal composite aerogels were obtained, which were respectively recorded as Sample 1, Sample 2, and Sample 3. The different specific parameters in the preparation process are shown in Table 1.

[0039] Table 1 (Specific parameters during the preparation of sample 1, sample 2 and sample 3)

[0040]

[0041] <Comparative Example>

[0042] In this comparative example, a composite aerogel is prepared as a comparison of Sample 1, Sample 2, and Sample 3 of the embodiment. The composite aerogel used as a comparison is recorded as a comparative sample. The preparation method of the comparative sample includes the following steps:

[0043] S01, prepare 2.11wt% graphene solution and 40mg / mL chitosan solution.

[0044] S02, using 12.75 mL of graphene solution as the substrate, a 20 mL CS / GO aerogel was prepared, to which 6.25 mL of chitosan solution was added to assist in the subsequent aerogel formation, and 1 mL of ethanol was added to enhance the surface tension.

[0045] S03, stirred for 3 h to ensure a uniform solution, stored in the freezer for 12 h, and freeze-dried for 24 h.

[0046] S04 was heated at 800 °C for 2 h in an Ar atmosphere to obtain a comparative sample.

[0047] <Test Example>

[0048] This test example uses X-ray diffraction (abbreviated as XRD, ) Determine the crystal structure of sample 1, sample 2, sample 3 and the control sample.

[0049] Figure 2 1 is the XRD pattern of sample 1, sample 2, sample 3 and the comparative sample in the test example of the present invention.

[0050] like Figure 2 As shown, sample 1, sample 2 and sample 3 have similar crystal structures, and the diffraction peak at 44.5° is identified as the (111) crystal plane of metallic Co (JCPDS: 15-0806), confirming the existence of magnetic Co metal. In addition, a broad peak is depicted near 2θ = 26°, which is related to the (002) crystal plane of graphitized carbon (JCPDS No. 75-1621). In addition, the intensity of the graphite peak increases from sample 1 to sample 2 and decreases from sample 2 to sample 3, indicating that the crystallinity of graphitized carbon peaks with increasing Co content. The results show that in an inert atmosphere, magnetic metal Co particles grow by reduction and nucleation of metal ions. Cobalt metal has a certain catalytic effect on the carbonization of organic ligands. The organic ligands are pyrolyzed and carbonized, and each carbon atom produced is carbonized with the sp in the carbon structure. 2 The three adjacent carbon atoms in the hybrid orbital are bonded. The XRD pattern shows that the control sample does not contain MXene phase components, while the magnetic metal composite aerogel of Co / C / MXene composite material was successfully prepared in the embodiment.

[0051] This test example also used a scanning electron microscope to observe the morphology of sample 1, sample 2, sample 3 and the comparison sample and performed energy spectrum detection.

[0052] Figure 3 1 is the SEM spectrum of sample 1, sample 2, sample 3 and the comparative sample in the test example of the present invention.

[0053] like Figure 3 As shown in the figure, the SEM images of sample 1, sample 2 and sample 3 are magnified at 200×. The morphology of the three samples all show a layered porous structure. The formula uses the same components, and although the component mass ratios are different, they still show relatively similar morphological characteristics. After 12 hours of freezing, ice crystals with a certain orientation pattern are formed in the graphene system solution, such as Figure 3 After 24 hours of freeze-drying, pores are formed after the ice crystals sublime. The layered structure of the sample added with MXene solution shows wrinkles on the surface. After adding the Co-NT composite, the three samples and the control sample all maintain the layered porous geometry, and the microstructure does not show obvious changes. However, the pore size varies with the content of the Co-NT composite, and the pores in Figure b are slightly reduced. The SEM image shows that the porous aerogel was successfully prepared in the embodiment. The microscopic morphology of the control sample is similar to that of the embodiment sample, both showing a layered porous structure and the presence of wrinkles, but its pore size is relatively large.

[0054] Depend on Figure 2 XRD patterns and Figure 3 The SEM images show that the embodiment successfully prepared a porous aerogel of Co / C / MXene composite material, that is, a magnetic metal composite aerogel.

[0055] In this test example, Sample 1, Sample 2, Sample 3, and the control sample were cut into square specimens with a length of 2.2 cm, a width of 1.1 cm, and a thickness of 0.4 cm. The electromagnetic parameters were then measured using a vector network analyzer in the frequency range of 8.2 GHz to 12.4 GHz, thereby providing an application of a magnetic metal composite aerogel in electromagnetic shielding.

[0056] Figure 4 EMI performance curves of sample 1, sample 2, sample 3 and the comparative sample in the test example of the present invention.

[0057] The layered porous characteristics of the material come from the composite skeleton of graphene. This structure can promote multiple reflections and scattering of electromagnetic waves inside the material, converting energy into heat and dissipating it, reducing the energy of electromagnetic waves passing through the material, and improving shielding effectiveness. In addition, through immersion in MXene solution, a layer of MXene two-dimensional nanomaterial is evenly attached to the internal cavity of the material; its internal transition metal carbide forms a conductive channel in the MXene structure, which helps to improve the migration of electrons and the conductivity. In addition, cobalt metal has high electrical conductivity and magnetic permeability. By adding an appropriate amount of Co magnetic particle composites, the electrical conductivity and magnetic properties of the material can be improved, and its conductivity to electromagnetic waves can be enhanced, thereby improving the shielding effect of the material. Figure 4 By optimizing each component, optimal shielding performance can be achieved. Specifically, the shielding performance of Samples 1, 2, and 3 is 31.7dB, 42.2dB, and 36.5dB, respectively. Therefore, compared to the 22.0dB shielding performance of the control sample, the samples prepared in the examples all achieved excellent shielding performance.

[0058] In summary, a simple chemical reaction and heat treatment process allows the preparation of metallic magnetic Co / graphene / MXene composite aerogels with varying properties, and the selection of components with superior electromagnetic shielding performance. These process parameters effectively control the physical phases of the Co / graphene / MXene composites and regulate their shielding properties, thus facilitating industrial production and having important implications for the development and widespread application of electromagnetic shielding materials.

[0059] Those skilled in the art will appreciate that the present invention is not limited to the foregoing embodiments. The foregoing embodiments and descriptions are merely illustrative of the principles of the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention. Such changes and modifications are intended to fall within the scope of the present invention. The scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a magnetic metal composite aerogel, characterized in that: The following steps are involved: S10, dissolving a cobalt salt and 2,5-dihydroxyterephthalic acid in a solvent to perform a hydrothermal reaction to obtain a cobalt metal organic framework; S20, carbonizing the cobalt metal organic framework to obtain a Co / C aerogel; S30, immersing the Co / C aerogel in a MXene solution to obtain the magnetic metal composite aerogel.

2. The method for preparing the magnetic metal composite aerogel according to claim 1, characterized in that: in, In step S10, the cobalt salt includes cobalt acetate tetrahydrate and / or cobalt chloride tetrahydrate, and the solvent includes any one or more of anhydrous ethanol, methanol or deionized water.

3. The method for preparing the magnetic metal composite aerogel according to claim 1 or 2, characterized in that: in, Step S10 includes the following sub-steps: S11, mixing the cobalt salt solution and the 2,5-dihydroxyterephthalic acid solution and stirring to obtain a reaction solution; S12, adding water to the reaction solution and performing a hydrothermal reaction to prepare a solution of the cobalt metal organic framework.

4. The method for preparing the magnetic metal composite aerogel according to claim 3, characterized in that: in, In step S11, the concentration of cobalt salt in the cobalt salt solution is 20-40 mg / mL, the concentration of 2,5-dihydroxyterephthalic acid in the 2,5-dihydroxyterephthalic acid solution is 2-10 mg / mL, the volume ratio of the cobalt salt solution to the 2,5-dihydroxyterephthalic acid solution is (1-8):(1-4), and the stirring time is 2 hours. In step S12, the volume ratio of the amount of water added to the reaction solution is (1-3):(1-9), and the hydrothermal reaction conditions are: heating to 50-180°C at a heating rate of 1°C / min-10°C / min and then keeping warm for 12h-24h.

5. The method for preparing the magnetic metal composite aerogel according to claim 1, characterized in that: in, Step S20 includes the following sub-steps: S21, mixing the cobalt metal organic framework and graphene in a solvent to prepare a Co / C composite material solution; S22, freeze-drying the Co / C composite material solution and heating it under an inert atmosphere to obtain the Co / C aerogel.

6. The method for preparing the magnetic metal composite aerogel according to claim 5, characterized in that: in, The mass of the cobalt metal organic framework in step S21 is recorded as m1, and the mass of the graphene is recorded as m2, m1:m2=1:(4-10), In step S22, the inert atmosphere is argon, and the heating method is: heating to 500°C to 900°C at a heating rate of 2°C / min to 10°C / min and then keeping the temperature for 60min to 180min.

7. The method for preparing the magnetic metal composite aerogel according to claim 5 or 6, characterized in that: in, In step S21, chitosan solution and ethanol are also added.

8. The method for preparing the magnetic metal composite aerogel according to claim 6, characterized in that: in, The immersion method in step S30 is: uniformly dripping the MXene solution onto the surface of the Co / C aerogel until the MXene solution precipitates from the bottom of the Co / C aerogel, and the Co / C aerogel is converted into a Co / C / MXene composite aerogel, that is, the magnetic metal composite aerogel. The mass of MXene in the MXene solution in step S30 is recorded as m3, m1:m3=1:(0.01-0.2).

9. A magnetic metal composite aerogel, characterized in that: The aerogel is prepared by the method for preparing the magnetic metal composite material according to any one of claims 1 to 8.

10. Application of the magnetic metal composite aerogel as claimed in claim 9 in electromagnetic shielding, in, The electromagnetic shielding performance of the magnetic metal composite aerogel is 20-50 dB.

Citation Information

Patent Citations

  • Three-dimensional graphene-coated metal-organic framework (MOF) composite electrode material and preparation method thereof

    CN107195875A

  • Cobalt-based MOFs material, and preparation method and application thereof

    CN107573233A

  • Metal organic framework composite aerogel material as well as preparation method and application thereof

    CN111282522A

  • Double-coating polyimide-based electromagnetic shielding composite aerogel and preparation method thereof

    CN114805919A

  • High-strength polyimide-based electromagnetic shielding composite aerogel and preparation method thereof

    CN114957990A