Perovskite-based catalyst with double functional sites, preparation method and application of perovskite-based catalyst in catalysis of chlorine-containing volatile organic pollutants
The perovskite-based catalyst was modified through sol-gel method and two-step acid treatment strategy to form a P-Co-LaCoO3 catalyst with dual functional sites, solving the low temperature of perovskite-based catalysts when catalyzing chlorine-containing volatile organic compounds. The problems of insufficient activity and poor anti-toxicity have achieved efficient and stable catalytic effects and environmental protection.
Patent Information
- Application Number
- CN202411123033.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing perovskite-based catalysts are insufficient in low-temperature activity, poor anti-toxicity ability and produce toxic by-products when catalyzing chlorine-containing volatile organic pollutants, and cannot last for industrial applications.
Using sol-gel method and two-step acid treatment strategy, the active sites of perovskite materials are activated by nitric acid treatment, and the acid sites are introduced through phosphoric acid modification to form a P-Co-LaCoO3 catalyst with bifunctional sites, and optimized their Redox capacity and chlorine resistance.
The catalyst is efficient and chlorine-resistant, and the conversion rate of degraded chlorine-containing volatile organic compounds reaches 90%, and the reaction activity is maintained at high temperature, reducing the generation of toxic by-products, and has good water resistance and thermal shock resistance. .
Smart Images

Figure CN119016074A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of air pollution control, and relates to a perovskite-based catalyst with dual functional sites, a preparation method and application thereof in catalyzing chlorine-containing volatile organic pollutants. Background Art
[0002] Volatile organic compounds (VOCs) are particulate matter in the atmosphere (PM 2.5 ) and ozone (O3), and its efficient control is an important issue in the field of air pollution control in my country at this stage.
[0003] VOCs generally refer to organic liquids and solids with a saturated vapor pressure greater than 70Pa at room temperature and a boiling point below 260°C at normal pressure. This type of compound is widely used in industrial fields such as packaging and printing, automotive spraying, synthetic leather, and rubber recycling. The main sources in the environment are incomplete combustion of fuels and waste incineration, organic emissions during chemical preparation (oil refining, petrochemicals, coatings, inks, adhesives, pesticides, and medicines), and volatile emissions during solvent use (printing and packaging, automotive spraying, furniture manufacturing, footwear manufacturing, and grain fumigation, etc.). It mainly includes alkanes, aromatic hydrocarbons, alkenes, halogenated hydrocarbons, esters, aldehydes, ketones, and others. In addition to some of the pollution characteristics of general VOCs, most chlorinated volatile organic compounds (CVOCs) have stable physical and chemical properties. Therefore, the pollution of this type of substance has become the focus and difficulty of research due to its high persistence, high mobility, and high toxicity.
[0004] At present, the commonly used disposal methods in industry can be divided into two categories: non-destructive (physical adsorption, condensation method, membrane separation, etc.) and destructive technology (direct combustion, catalytic combustion, biodegradation, etc.). Among various CVOCs treatment and disposal technologies, low-temperature catalytic combustion is considered to be an economical and reliable CVOCs disposal method due to its advantages such as low ignition temperature, high reaction activity, and controllable selectivity. The core of this method is the design of the catalyst. Traditional precious metal-based catalysts are widely used in the catalytic destruction of CVOCs and exhibit excellent catalytic activity. However, due to the presence of Cl, precious metal-based catalysts usually encounter problems such as the generation of toxic chlorine by-products and catalyst deactivation due to chloride poisoning, coking, and competitive adsorption of water, making them unable to operate for a long time in industrial applications.
[0005] Perovskite-based catalysts are very suitable for thermal catalysis under actual working conditions (water vapor, thermal shock, chlorine poisoning) due to their excellent structural stability and thermal stability. However, due to their small specific surface area and poor redox ability, the performance of pure perovskite-based catalysts in the catalytic destruction of CVOCs is not ideal (high complete destruction temperature and poor chlorine resistance). Therefore, the development of an efficient and reliable industrial catalyst for the catalytic destruction of CVOCs has become one of the key issues that need to be solved urgently. Summary of the invention
[0006] In order to overcome the problems of insufficient low-temperature activity, poor anti-poisoning ability and generation of toxic by-products in existing perovskite-based catalysts, the purpose of the present invention is to provide a perovskite-based catalyst with a dual-functional site, a preparation method and its application in catalyzing chlorine-containing volatile organic pollutants. The perovskite-based catalyst with a dual-functional site prepared by the method exhibits good low-temperature activity, chlorine resistance and product selectivity, thereby achieving high catalytic efficiency, strong anti-poisoning ability and low by-product production while realizing its environmentally friendly characteristics.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a perovskite-based catalyst having a dual-functional site comprises the following steps:
[0009] Adding citric acid and a modifier to a solution containing lanthanum salt and cobalt salt, and heating to generate a gel;
[0010] The gel is aged and then calcined to obtain a powder;
[0011] The powder is dispersed in a nitric acid solution, separated, and dried to obtain a dried powder, and the dried powder is then dispersed in a phosphoric acid solution, separated, and dried to obtain a perovskite-based catalyst with dual functional sites.
[0012] Furthermore, the lanthanum salt is lanthanum nitrate, and the cobalt salt is cobalt nitrate.
[0013] Furthermore, the mass ratio of lanthanum salt to cobalt salt is 4.3-10.8:2.9-7.3.
[0014] Furthermore, the mass ratio of citric acid to cobalt salt is 4.2-10.5:2.9-7.3.
[0015] Furthermore, the modifier is ethylene glycol, and the mass ratio of the modifier to the cobalt salt is 0.8-2.1:2.9-7.3.
[0016] Furthermore, the aging process is: aging at 120-130°C for 12-15h; the roasting process is: first roasting at 350-400°C for 3-4h, and then roasting at 750-850°C for 3-4h.
[0017] Furthermore, the concentration of the nitric acid solution is 1 mol / L, the dispersion time is 30 minutes, and the concentration of the phosphoric acid solution is 0.1 mol / L, the dispersion time is 40-50 minutes.
[0018] A perovskite-based catalyst with dual functional sites.
[0019] Application of a perovskite-based catalyst with dual functional sites in the catalytic decomposition of chlorinated volatile organic pollutants.
[0020] Furthermore, in the case of m-dichlorobenzene, the reaction space velocity is 20000-30000 mL·h -1 ·g -1 , under the condition of oxygen concentration of 10-21%, the catalyst degrades m-dichlorobenzene at 150-450°C.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention adopts a two-step acid treatment strategy, firstly reconstructing the surface of the perovskite material to expose sufficient active sites and activate lattice oxygen to optimize its redox ability, and then modifying the material surface with phosphoric acid to introduce rich Acidic sites increase the surface acidity of the material, thereby activating the synergistic effect between the surface active sites and acidic sites. Compared with the modification strategy of traditional perovskite-based catalysts, the two-step acid treatment modification strategy takes into account the redox ability and surface acidity of the catalyst, and achieves efficient and stable destruction of CVOCs through the synergistic effect between active sites and acidic sites. In addition, the modification method is simple and convenient, takes a short time, and saves time and energy.
[0023] The P-Co-LaCoO3 perovskite catalyst prepared by the present invention exhibits good low-temperature reduction performance, excellent chlorine resistance, water resistance and thermal shock resistance in the degradation of m-dichlorobenzene. -1 ·g -1Under the conditions of , the conversion rate reached 90% at 350℃, and the reaction lasted for 30 hours, and the conversion rate remained at about 80%, indicating that the catalyst has excellent catalytic activity and chlorine resistance. After reacting at 500℃ for 30 hours, there was no deactivation phenomenon, indicating that the catalyst has strong resistance to thermal shock. In addition, the catalytic activity increased by 15% after the introduction of 5vol.% water vapor, and the output of toxic by-products was only 10% of that under dry conditions, indicating that the catalyst has excellent water resistance, and the presence of water vapor promotes the conversion of meta-dichlorobenzene and inhibits the generation of toxic by-products. The catalyst has the advantages of low cost, good low-temperature activity, strong water resistance, good anti-poisoning ability, high by-product selectivity, etc., and has important application prospects in the field of low-temperature purification of chlorine-containing volatile organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the temperature-programmed reduction (H2-TPR) curve of the perovskite-based catalyst with dual functional sites in the present invention;
[0025] Figure 2 This is the temperature-programmed desorption (NH3-TPD) curve of the perovskite-based catalyst with dual functional sites in the present invention;
[0026] Figure 3 This is the element valence state distribution (XPS) curve of O1s of the perovskite-based catalyst with dual functional sites in the present invention;
[0027] Figure 4 This is an activity test curve of the perovskite-based catalyst with dual functional sites in the present invention for catalytic degradation of m-dichlorobenzene;
[0028] Figure 5 This is a stability test curve of the perovskite-based catalyst with dual functional sites in the present invention for catalytic degradation of m-dichlorobenzene;
[0029] Figure 6 This is a test curve of thermal shock resistance of the perovskite-based catalyst with dual functional sites in the present invention for catalytic degradation of m-dichlorobenzene;
[0030] Figure 7 This is a test curve of water resistance of the perovskite-based catalyst with dual functional sites in the present invention for catalytic degradation of m-dichlorobenzene;
[0031] Figure 8 This is the byproduct distribution curve when testing the water resistance of the perovskite-based catalyst with dual functional sites in the present invention for catalytic degradation of m-dichlorobenzene. DETAILED DESCRIPTION
[0032] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0033] The present invention utilizes a sol-gel method and acid treatment to prepare a multifunctional perovskite-based catalyst P-Co-LaCoO3 for synergistically treating chlorinated volatile organic compounds. The present invention mainly uses a two-step acid treatment modification strategy to directionally anchor phosphate groups on the surface lanthanum sites, and combines nitric acid selective etching to increase the content of surface defects, activate the synergistic effect between active sites and acid sites, and improve its low-temperature oxidation activity and anti-poisoning ability. The perovskite-based catalyst successfully generates different functional centers on the surface of the material through a two-step acid treatment modification strategy, making it an effective degradation material for chlorinated volatile organic pollutants. The specific steps are as follows:
[0034] (1) Dissolve 4.3-10.8 g of lanthanum nitrate in 40-100 mL of deionized water and stir at 600-800 r / min for 40 min at room temperature until it is completely dissolved and a clear and transparent solution is formed;
[0035] (2) dissolving 2.9-7.3 g of cobalt nitrate in the clear solution obtained in step (1), stirring at 600-800 r / min for 40 min at room temperature until it is completely dissolved and a clear and transparent solution is formed, and heating to 90° C.;
[0036] (3) dissolving 4.2-10.5 g of citric acid in the heated clear solution obtained in step (2), stirring at 90° C. at 600-800 r / min for 60 min until it is completely dissolved and a clear and transparent solution is formed, and then cooling to 80° C.;
[0037] (4) adding 0.8-2.1 g of ethylene glycol (modifier) dropwise to the solution of step (3), and stirring at 80° C. and 600-800 r / min for 8 h after the addition is complete to allow the solution to fully react and form a gel;
[0038] (5) placing the gel obtained in step (4) in an oven at 120-130° C. for aging for 12-15 hours to obtain a precursor;
[0039] (6) calcining the precursor obtained in step (5) in a muffle furnace at 350-400° C. for 2-4 h, and then heating to 750-850° C. for 3-4 h to obtain a black solid powder;
[0040] (7) 2 g of the black powder obtained in step (6) was redispersed in 40 mL of 1 mol / L nitric acid solution and stirred at 600-800 r / min for 30 min at room temperature;
[0041] (8) The solution obtained in step (7) was then filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the obtained black powder was placed in a vacuum drying oven at 60° C. and dried for 10 h until the obtained powder was dry;
[0042] (9) Redisperse 1 g of the black powder obtained in step (8) in 60 mL of 0.1 mol / L phosphoric acid solution and perform ultrasonic treatment for 40-50 min;
[0043] (10) The solution of step (9) was then filtered under vacuum conditions and washed with deionized water and anhydrous ethanol several times to obtain a black powder. The obtained black powder was then placed in a vacuum drying oven at 60° C. and dried for 10 h until the obtained powder was dry, thereby finally obtaining a catalyst.
[0044] The catalyst prepared by the present invention is treated with nitric acid to selectively etch the surface metal elements, expose more surface active sites, and activate the lattice oxygen on the catalyst surface, so the material has excellent low-temperature redox ability and abundant active sites.
[0045] The catalyst prepared by the present invention is treated with phosphoric acid so that the phosphate radical can be directionally anchored on the lanthanum site, so the surface of the material has abundant acid sites.
[0046] The catalyst prepared by the present invention activates the synergistic effect between the active site and the acidic site through two-step acid treatment. The Co3O4 exposed on the surface of the material mainly provides low-temperature reduction active sites and achieves deep oxidation of target pollutants in the system, while the La element mainly provides phosphate anchoring sites and promotes the transfer and removal of chlorine elements. The mutual synergy between the two functional sites simultaneously promotes the deep oxidation of m-dichlorobenzene.
[0047] The invention discloses a method for preparing a perovskite-based catalyst having dual functional sites for catalyzing the decomposition of chlorinated volatile organic pollutants, specifically, a method for preparing a perovskite-based catalyst having dual functional sites for catalyzing the decomposition of chlorinated volatile organic pollutants at a reaction space velocity of 20,000 to 30,000 mL·h -1 ·g -1 , under the condition of oxygen concentration of 10-21%, 90% degradation of intermediate dichlorobenzene in industrial typical CVOCs can be achieved at around 350°C.
[0048] Example 1 Preparation of a perovskite-based catalyst with dual functional sites by sol-gel method and acid treatment
[0049] Dissolve 7.58g of lanthanum nitrate and 5.09g of cobalt nitrate in 70mL of deionized water, stir at 600r / min for 40min at room temperature until completely dissolved and a clear and transparent solution is formed, and heat the solution to 90°C first; then add 7.35g of citric acid, stir at 90°C at 600r / min for 60min until completely dissolved and a clear and transparent solution is formed, then cool to 80°C; then add 1.45g of ethylene glycol dropwise, stir at 80°C at 600r / min for 8h to promote the solution to fully react and form a gel. Put the gel in an oven and age it at 120°C for 12h to obtain a precursor, then the precursor is calcined at 350°C in a muffle furnace for 2h, then heated to 800°C and calcined for 3h to obtain a black solid powder. Subsequently, 2g of the black powder was redispersed in 40mL of 1mol / L nitric acid solution, stirred at 800r / min for 30min at room temperature, and then the obtained liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain black powder, and then the obtained black powder was placed in a vacuum drying oven at 60°C for 10h until the obtained powder was dry. 1g of the prepared dry powder was redispersed in 60mL of 0.1mol / L phosphoric acid solution, ultrasonically treated for 40min, and then the obtained liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain black powder, and then the obtained black powder was placed in a vacuum drying oven at 60°C for 10h until the obtained powder was dry, and finally a perovskite-based catalyst with dual functional sites, namely P-Co-LaCoO3 oxide, was obtained.
[0050] See also Figure 1 As can be seen from the figure, the perovskite-based catalyst with dual functional sites showed a reducible peak at 283°C, indicating that the material has excellent low-temperature reducible properties and has great advantages in the field of catalytic oxidation.
[0051] See also Figure 2 It can be seen that the perovskite-based catalyst with dual functional sites showed an ammonia desorption peak at 201°C, indicating that the material has excellent weak acidic properties and has a good inhibitory effect on polychlorinated by-products during the catalytic oxidation of chlorinated volatile organic compounds.
[0052] See also Figure 3 , it can be seen that the surface of the perovskite-based catalyst with dual functional sites contains abundant surface adsorbed oxygen (531.2 eV), which can promote the deep oxidation of chlorinated volatile organic pollutants.
[0053] The catalyst prepared by the present invention has a large specific surface area (50.74m 2 ·g -1 ) and pore volume (0.274cm 3 ·g -1), which can effectively promote the transmission of target pollutants on the surface of catalytic materials;
[0054] Example 2 Activity test and evaluation of the catalytic degradation of m-dichlorobenzene by perovskite-based catalysts with dual functional sites
[0055] The solid powder obtained in Example 1 was tableted and sieved (40-60 mesh), and 0.3 g of the sieved catalyst was accurately weighed. Meta-dichlorobenzene was used as the probe gas, the concentration of the reactant was controlled at 500 ppm, and the reaction space velocity was 20000 mL·h -1 ·g -1 Under the condition of oxygen concentration of 21%, the catalytic reaction activity of the catalyst at different temperatures (150, 200, 250, 300, 350, 380, 400, 430 and 450° C.) was tested respectively, and the reaction products were monitored and analyzed by gas chromatography.
[0056] See also Figure 4 It can be seen that the perovskite-based catalyst with dual functional sites has good low-temperature catalytic performance at 350 °C and a reaction space velocity of about 20000 mL·h -1 ·g -1 Under these conditions, 90% conversion of m-dichlorobenzene can be achieved, which can basically be applied to the current industrial catalytic RCO catalytic reaction device and can achieve good results.
[0057] Example 3 Test on the stability and thermal shock resistance of the perovskite-based catalyst with dual functional sites for catalytic degradation of m-dichlorobenzene
[0058] The solid powder obtained in Example 1 was pressed into tablets and sieved (40-60 mesh). 0.3 g of the sieved catalyst was accurately weighed and placed in the fixed bed of the evaluation device. Meta-dichlorobenzene was used as the probe gas. The concentration of the reactant was controlled at 500 ppm and the reaction space velocity was 20000 mL·h -1 ·g -1 The oxygen concentration was 21%, and the catalytic reaction activity of the catalyst was continuously tested at 350°C and 500°C. The reaction products were monitored and analyzed by gas chromatography.
[0059] See also Figure 5 It can be seen that the perovskite-based catalyst with dual functional sites has a high reaction temperature at 350 °C and a reaction space velocity of about 20000 mL·h -1 ·g -1 Under the above conditions, within 30 hours, the conversion rate of m-dichlorobenzene by the catalyst was maintained at about 80%, showing excellent oxidation stability of chlorinated volatile organic compounds. Figure 6 It can be seen that the perovskite-based catalyst with dual functional sites has a high reaction speed of about 20000 mL·h at 500 °C. -1 ·g -1Under the above conditions, within 30 hours, the conversion rate of the catalyst to m-dichlorobenzene remained at about 100%, showing very excellent thermal shock resistance.
[0060] Example 4 Analysis of the intermediates of the degradation of m-dichlorobenzene by perovskite-based catalysts with dual functional sites
[0061] The solid powder obtained in Example 1 was tableted and sieved (40-60 mesh), and 0.3 g of the sieved catalyst was accurately weighed. Meta-dichlorobenzene was used as the probe gas, the concentration of the reactant was controlled at 500 ppm, and the reaction space velocity was 20000 mL·h -1 ·g -1 , the oxygen concentration was 21%, and the intermediate product production of the catalyst at different temperatures (150, 200, 250, 300, 350, 380, 400, 430 and 450°C) was tested respectively. The reaction products were monitored and analyzed by gas chromatography and in-situ online mass spectrometry.
[0062] Example 5 Water resistance test and intermediate product analysis of the degradation of m-dichlorobenzene by perovskite-based catalyst with dual functional sites
[0063] The solid powder obtained in Example 1 was pressed into tablets and sieved (40-60 mesh). 0.3 g of the sieved catalyst was accurately weighed and placed in the fixed bed of the evaluation device. Meta-dichlorobenzene was used as the probe gas. The concentration of the reactant was controlled at 500 ppm. Different concentrations of water vapor (1, 2 and 5 vol.%) were introduced. The reaction space velocity was 20000 mL·h -1 ·g -1 The oxygen concentration was 21%, and the catalytic reaction activity of the catalyst was continuously tested at 350° C. The reaction products were monitored and analyzed by gas chromatography.
[0064] See also Figure 7 It can be seen that the perovskite-based catalyst with dual functional sites has a high reaction temperature at 350 °C and a reaction space velocity of about 20000 mL·h -1 ·g -1 Under the above conditions, within 30 hours, water vapor of different concentrations can improve the conversion rate of the catalyst to m-dichlorobenzene, and the catalytic activity is increased from 80% to 95% when 5 vol.% water vapor is introduced. The catalyst exhibits very excellent water resistance.
[0065] See also Figure 8 It can be seen that the perovskite-based catalyst with dual functional sites has a high reaction temperature at 350 °C and a reaction space velocity of about 20000 mL·h -1 ·g -1Under the above conditions, within 30 hours, different concentrations of water vapor can significantly inhibit the formation of by-products. When 5 vol.% of water vapor is introduced, the amount of by-products generated is only 10% of that under dry conditions, indicating that the water vapor present in actual working conditions has a significant promoting effect on the catalytic degradation of m-dichlorobenzene by the catalyst.
[0066] Example 6
[0067] Dissolve 4.3g of lanthanum nitrate and 2.9g of cobalt nitrate in 80mL of deionized water, stir at 600r / min for 40min at room temperature until completely dissolved and a clear and transparent solution is formed, and heat the solution to 90°C first; then add 4.2g of citric acid, stir at 90°C at 800r / min for 60min until completely dissolved and a clear and transparent solution is formed, then cool to 80°C; then add 0.8g of ethylene glycol dropwise, stir at 80°C at 800r / min for 8h to promote the solution to fully react and form a gel. Put the gel in an oven and age at 120°C for 15h to obtain a precursor, then the precursor is calcined at 350°C in a muffle furnace for 4h, then heated to 770°C and calcined for 3h to obtain a black solid powder. Subsequently, 2g of the black powder was redispersed in 40mL of 1mol / L nitric acid solution, stirred at 600r / min for 30min at room temperature, and then the obtained liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain black powder, and then the obtained black powder was placed in a vacuum drying oven at 60°C for 10h until the obtained powder was dry. The prepared 1g dry powder was redispersed in 60mL of 0.1mol / L phosphoric acid solution, ultrasonically treated for 40min, and then the obtained liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain black powder, and then the obtained black powder was placed in a vacuum drying oven at 60°C for 10h until the obtained powder was dry, and finally a perovskite-based catalyst with dual functional sites was prepared.
[0068] Example 7
[0069] Dissolve 10.8g of lanthanum nitrate and 7.3g of cobalt nitrate in 100mL of deionized water, stir at 800r / min for 40min at room temperature until completely dissolved and a clear and transparent solution is formed, and first heat the solution to 90°C; then add 10.5g of citric acid, stir at 90°C at 600r / min for 60min until completely dissolved and a clear and transparent solution is formed, then cool to 80°C; then add 2.1g of ethylene glycol dropwise, stir at 80°C at 600r / min for 8h to promote the solution to fully react and form a gel. Put the gel in an oven and age it at 130°C for 12h to obtain a precursor, then the precursor is calcined at 400°C in a muffle furnace for 2h, then heated to 750°C and calcined for 4h to obtain a black solid powder. Subsequently, 2 g of the black powder was redispersed in 40 mL of 1 mol / L nitric acid solution, stirred at 800 r / min for 30 min at room temperature, and then the resulting liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the resulting black powder was placed in a vacuum drying oven at 60 ° C for 10 h until the powder was dry. 1 g of the prepared dry powder was redispersed in 60 mL of 0.1 mol / L phosphoric acid solution, ultrasonically treated for 50 min, and then the resulting liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the resulting black powder was placed in a vacuum drying oven at 60 ° C for 10 h until the powder was dry, and finally a perovskite-based catalyst with dual functional sites was obtained.
[0070] Example 8
[0071] Dissolve 6.5g of lanthanum nitrate and 4.4g of cobalt nitrate in 60mL of deionized water, stir at 700r / min for 40min at room temperature until completely dissolved and a clear and transparent solution is formed, and heat the solution to 90°C first; then add 6.3g of citric acid, stir at 90°C at 700r / min for 60min until completely dissolved and a clear and transparent solution is formed, then cool to 80°C; then add 1.2g of ethylene glycol dropwise, stir at 80°C at 700r / min for 8h to promote the solution to fully react and form a gel. Put the gel in an oven and age at 125°C for 13h to obtain a precursor, then the precursor is calcined at 370°C in a muffle furnace for 3h, then heated to 850°C and calcined for 3h to obtain a black solid powder. Subsequently, 2 g of the black powder was redispersed in 40 mL of 1 mol / L nitric acid solution, stirred at 700 r / min for 30 min at room temperature, and then the resulting liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the resulting black powder was placed in a vacuum drying oven at 60 ° C for 10 h until the powder was dry. The prepared 1 g of dry powder was redispersed in 60 mL of 0.1 mol / L phosphoric acid solution, ultrasonically treated for 45 min, and then the resulting liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the resulting black powder was placed in a vacuum drying oven at 60 ° C for 10 h until the powder was dry, and finally a perovskite-based catalyst with dual functional sites was prepared.
[0072] Example 9
[0073] Dissolve 9.7g of lanthanum nitrate and 6.5g of cobalt nitrate in 100mL of deionized water, stir at 650r / min for 40min at room temperature until completely dissolved and a clear and transparent solution is formed, and heat the solution to 90°C first; then add 9.5g of citric acid, stir at 750r / min at 90°C for 60min until completely dissolved and a clear and transparent solution is formed, then cool to 80°C; then add 1.9g of ethylene glycol dropwise, stir at 80°C at 800r / min for 8h to promote the solution to fully react and form a gel. Put the gel in an oven and age at 125°C for 14h to obtain a precursor, then the precursor is calcined at 380°C in a muffle furnace for 2h, then heated to 800°C and calcined for 3h to obtain a black solid powder. Subsequently, 2 g of the black powder was redispersed in 40 mL of 1 mol / L nitric acid solution, stirred at 800 r / min for 30 min at room temperature, and then the resulting liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the resulting black powder was placed in a vacuum drying oven at 60 ° C for 10 h until the powder was dry. 1 g of the prepared dry powder was redispersed in 60 mL of 0.1 mol / L phosphoric acid solution, ultrasonically treated for 40 min, and then the resulting liquid was filtered under vacuum conditions, and washed with deionized water and anhydrous ethanol several times to obtain a black powder, and then the resulting black powder was placed in a vacuum drying oven at 60 ° C for 10 h until the powder was dry, and finally a perovskite-based catalyst with dual functional sites was prepared.
[0074] The perovskite-based catalyst with dual functional sites prepared by the present invention is synthesized by a sol-gel method, and modified by a two-step acid treatment strategy. The nitric acid treatment exposes sufficient active sites (Co) on the surface of the perovskite material, and then phosphoric acid modification anchors phosphate groups at the surface lanthanum sites, and the prepared catalyst P-Co-LaCoO3 is applied to the catalytic degradation of CVOCs. The material preparation method of the present invention is simple, economical, and easy to operate. The synergistic effect between the surface acid sites and the active sites is used to effectively degrade CVOCs under low temperature conditions, reduce the energy consumption of the reaction process, and promote the desorption of toxic species adsorbed on the surface of the material during the reaction, inhibit the generation of toxic by-products, realize the economic and environmentally friendly catalytic concept, and have good industrial application prospects.
[0075] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0076] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A method for preparing a perovskite-based catalyst having a dual-functional site, characterized in that: The following steps are involved: Adding citric acid and a modifier to a solution containing lanthanum salt and cobalt salt, and heating to generate a gel; The gel is aged and then calcined to obtain a powder; The powder is dispersed in a nitric acid solution, separated, and dried to obtain a dried powder, and the dried powder is then dispersed in a phosphoric acid solution, separated, and dried to obtain a perovskite-based catalyst with dual functional sites.
2. The method for preparing a perovskite-based catalyst having a dual-functional site according to claim 1, characterized in that: The lanthanum salt is lanthanum nitrate, and the cobalt salt is cobalt nitrate.
3. The method for preparing a perovskite-based catalyst having a dual-functional site according to claim 2, characterized in that: The mass ratio of lanthanum salt to cobalt salt is 4.3-10.8:2.9-7.
3.
4. The method for preparing a perovskite-based catalyst having a dual-functional site according to claim 1, characterized in that: The mass ratio of citric acid to cobalt salt is 4.2-10.5:2.9-7.
3.
5. The method for preparing a perovskite-based catalyst having dual functional sites according to claim 1, characterized in that: The modifier is ethylene glycol, and the mass ratio of the modifier to the cobalt salt is 0.8-2.1:2.9-7.
3.
6. The method for preparing a perovskite-based catalyst having dual functional sites according to claim 1, characterized in that: The aging process is: aging at 120-130°C for 12-15h; the roasting process is: first roasting at 350-400°C for 3-4h, and then roasting at 750-850°C for 3-4h.
7. The method for preparing a perovskite-based catalyst having dual functional sites according to claim 1, characterized in that: The concentration of the nitric acid solution is 1 mol / L, and the dispersion time is 30 minutes. The concentration of the phosphoric acid solution is 0.1 mol / L, and the dispersion time is 40-50 minutes.
8. A perovskite-based catalyst having dual functional sites prepared according to the method according to any one of claims 1 to 7.
9. Use of a perovskite-based catalyst having dual functional sites prepared according to the method of any one of claims 1 to 7 in catalyzing chlorine-containing volatile organic pollutants.
10. A use according to claim 9, characterized in that The reaction space velocity in m-dichlorobenzene is 20000~30000mL·h -1 ·g -1 , under the condition of oxygen concentration of 10-21%, the catalyst degrades m-dichlorobenzene at 150-450°C.
Citation Information
Patent Citations
Double-perovskite composite metal oxide catalyst and preparation method and application thereof
CN106475105A
Modified perovskite type catalyst and preparation method thereof
CN110026185A
Phosphorylated perovskite type catalyst as well as preparation method and application thereof
CN112604700A
Cobalt-based perovskite oxide catalyst and preparation and application thereof
CN116459840A
Source solution for formation of rerovskite type or bi sheet perovskite type oxide thin film, method of forming perovskite type or bi sheet perovskite oxide thin film, and perovskite type or bi sheet perovskite type oxide thin film