Silicon-aluminum material and preparation method thereof

By preparing silicon-aluminum materials with step-by-step pore distribution and high B acid content, the problems of pore limitation and insufficient acidity in traditional molecular sieve materials in residual oil hydrogenation process are solved, and the efficient catalytic effect in heavy oil hydrogenation process is achieved.

CN119038570AActive Publication Date: 2024-11-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310579856.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-29
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

Traditional molecular sieve materials have insufficient pore channel limitation and acidity in catalytic residue hydrogenation process, resulting in insufficient catalytic activity and inability to effectively crack thick ring aromatic hydrocarbons, limiting their application in heavy oil hydrogenation process.

Method used

Prepare a silicon-aluminum material with step-by-step channel distribution and high B acid content, mixing silicon source, additives and water to form a sol, perform heat treatment and hydrothermal treatment, combine acidic and alkaline aluminum-containing compounds to react, and regulate pH and temperature , forming a silicon-aluminum material with high pore volume and mesoporous-macroporous structure.

Benefits of technology

It achieves suitable pore structure and high acidity, improves catalytic activity, and is especially suitable for heavy oil hydrocracking processes, enhances the cracking capacity of densely cyclic aromatic hydrocarbons, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038570A_ABST
    Figure CN119038570A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-aluminum material and a preparation method thereof. After being roasted at 500-700 DEG C, the silicon-aluminum material has the following properties: the content of silicon dioxide is 20-40wt%, the pore volume is not less than 0.70 mL / g, and the specific surface area is 280-400m < 2 > / g. The preparation method of the silicon-aluminum material comprises the following steps: (1) uniformly mixing a first silicon source, a first auxiliary agent and water to obtain sol; (2) mixing the sol with alcohol, and carrying out heat treatment to obtain a first material flow; (3) reacting a second silicon source, an acidic aluminum-containing compound and an alkaline aluminum-containing compound to obtain a mixed solution; (4) mixing the mixed solution with a second auxiliary agent to obtain slurry; and (5) mixing the slurry and the first material flow, carrying out hydrothermal treatment, and then washing, drying and roasting to obtain the silicon-aluminum material. The silicon-aluminum material has the characteristics of molecular sieves, has stepped pore channel distribution, has the characteristic of high B acid content, and is suitable for being used as a catalytic material carrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic materials and relates to a silicon-aluminum material and a preparation method thereof. Background Art

[0002] Molecular sieve materials are widely used in petroleum refining, especially in hydrocracking process, due to their strong acid centers and high reactivity. However, with the continuous exploitation of traditional light oil, the reserves are decreasing, resulting in increasing dependence on oil resources such as residual oil.

[0003] However, the pores of molecular sieves are relatively small, while the residual oil raw materials have the characteristics of large molecules and high impurity content. The pore restriction effect on large molecules such as residual oil is relatively obvious, which easily leads to coking and blockage of the pores, thereby causing rapid deactivation. It is not suitable for the catalytic reaction of large molecules such as residual oil, which limits its application in the residual oil hydrogenation process. Macroporous silica-alumina materials have suitable pore structures and good hydrothermal stability. They also have B acid centers and L acid centers, and have certain cracking capabilities. They are particularly suitable for residual oil hydrocracking processes. However, the macroporous silica-alumina materials prepared by conventional methods are usually not acidic enough, which is not conducive to catalyzing the breakage of polycyclic aromatic hydrocarbons.

[0004] CN201710382457.7 discloses a highly active silicon-aluminum material and a method for manufacturing the same. The active silicon-aluminum material contains 15-45% silicon and 55-85% aluminum by weight of oxide, a total BET specific surface area of ​​300-500 m2 / g, a micropore specific surface area of ​​≯8% of the total BET specific surface area, and an average pore size of 5-18 nm; c represents the Al / Si atomic ratio of the material surface measured by the XPS method, and d represents the Al / Si atomic ratio of the material bulk phase measured by the XRF method, and c / d=1.2-1.9.

[0005] CN201710382466.6 discloses a porous silicon-aluminum material and a preparation method thereof. A porous silicon-aluminum material, characterized in that a diffuse diffraction peak appears at a 2θ angle of about 25° to 27° in the XRD spectrum of the material, and a trace amount of FAU crystal phase structure exists at the same time. In the chemical composition calculated by weight of oxides, silicon is 50 to 80%, aluminum is 20 to 50%, the average pore size is 20 to 50 nm, and the total specific surface area is ≯250 m 2 / g, wherein the proportion of micropore specific surface area in the total specific surface area is ≯28%; when the surface Al / Si atomic ratio measured by the XPS method is a, and the bulk Al / Si atomic ratio measured by the XRF method is b, a / b=1.2~1.7. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the main purpose of the present invention is to provide a silicon-aluminum material and a preparation method thereof. The silicon-aluminum material exhibits molecular sieve characteristics, has a stepped pore distribution, and has a high content of B acid, and is suitable for use as a catalytic material carrier, especially suitable for use as a carrier of a heavy oil hydrogenation catalyst.

[0007] The first aspect of the present invention provides a silicon-aluminum material, which has the following properties after being calcined at 500-700°C: a silicon dioxide content of 20-40wt%, preferably 25-35wt%; a pore volume of not less than 0.70mL / g, preferably greater than 0.80mL / g, generally 0.70-1.5mL / g; a specific surface area of ​​280-400m 2 / g, preferably 300 to 400 m 2 / g.

[0008] Further, in the silicon-aluminum material, as a preferred embodiment, the calcined form of the silicon-aluminum material after calcination has an XRD pattern as shown in the following table;

[0009] 2θ d-spacing, nm Relative Strength 7.9 0.08-0.12 VS 8.8 0.06-0.10 S 24.5 0.22-0.26 VS

[0010] The intensity value of the strongest diffraction peak in the XRD spectrum is defined as 100, then W represents weak, that is, relative intensity >0 to ≤20, M represents medium, that is, relative intensity >20 to ≤40, S represents strong, that is, relative intensity >40 to ≤60, and VS represents very strong, that is, relative intensity >60 to ≤100.

[0011] Furthermore, in the silicon-aluminum material, as a preferred embodiment, in the nuclear magnetic resonance aluminum spectrum of the silicon-aluminum material, there are strong absorption peaks near the chemical shifts of 59 ppm and 7 ppm.

[0012] Furthermore, in the silicon-aluminum material, as a preferred embodiment, in the nuclear magnetic resonance silicon spectrum of the silicon-aluminum material, there is a strong absorption peak near the chemical shift of -88 ppm and a weak absorption peak at -111 ppm.

[0013] Furthermore, in the silicon-aluminum material, as a preferred embodiment, the B acid content of the silicon-aluminum material is greater than 0.10 mmol / g, preferably 0.10 to 0.3 mmol / g, and more preferably 0.15 to 0.30 mmol / g.

[0014] Furthermore, in the silicon-aluminum material, as a preferred embodiment, the ratio of B acid to L acid in the silicon-aluminum material is 0.5 to 1.2, preferably 0.5 to 1.0.

[0015] Furthermore, in the silicon-aluminum material, as a preferred embodiment, the pore size distribution of the silicon-aluminum material has the following characteristics: the pore volume of pores with a pore diameter of less than 10 nm accounts for ≤15% of the total pore volume, the pore volume of pores with a pore diameter of 10-50 nm accounts for 50%-80% of the total pore volume, and the pore volume of pores with a pore diameter of >50 nm accounts for 5-35% of the total pore volume; preferably, the pore volume of pores with a pore diameter of less than 10 nm accounts for ≤10% of the total pore volume, the pore volume of pores with a pore diameter of 10-50 nm accounts for 60%-80% of the total pore volume, and the pore volume of pores with a pore diameter of >50 nm accounts for 10-30% of the total pore volume.

[0016] Furthermore, in the silicon-aluminum material, as a preferred embodiment, the Na2O content of the silicon-aluminum material is less than 0.5wt%, preferably less than 0.3wt%.

[0017] A second aspect of the present invention provides a method for preparing a silicon-aluminum material, the preparation method comprising the following steps:

[0018] (1) mixing a first silicon source, a first auxiliary agent and water under mixing conditions to obtain a sol;

[0019] (2) mixing the sol obtained in step (1) with alcohol and then heat treating it to obtain a first stream;

[0020] (3) adding a second silicon source, an acidic aluminum-containing compound, and a basic aluminum-containing compound into a reactor containing bottom water under contact conditions to obtain a mixed solution after reaction;

[0021] (4) mixing the mixed solution obtained in step (3) with a second auxiliary agent under contact conditions to obtain a slurry;

[0022] (5) Under contact conditions, the slurry obtained in step (4) and the first stream obtained in step (2) are mixed and hydrothermally treated, and after the treatment, the silicon-aluminum material is obtained by washing, drying and roasting.

[0023] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the first silicon source in step (1) is one or more of tetraethyl orthosilicate, methyl orthosilicate, and silica sol, preferably tetraethyl orthosilicate.

[0024] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the first auxiliary agent in step (1) can be one or more of tetrapropylammonium hydroxide and tetrapropylammonium bromide; preferably, it is tetrapropylammonium hydroxide.

[0025] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the alcohol in step (2) is a C1-C3 alcohol, which can be one or more of a monohydric alcohol, a dihydric alcohol, or a polyhydric alcohol; the specific alcohol can be one or more of ethanol, ethylene glycol, and propylene glycol, preferably propylene glycol.

[0026] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the mass ratio of the first silicon source, the first auxiliary agent, water and alcohol is 3-6:5-8:2-4:0.5-5.

[0027] Furthermore, in the above-mentioned method for preparing silicon aluminum material, as a specific embodiment, the heat treatment temperature in step (2) is 60-100° C., preferably 80-100° C.; the treatment time is not more than 24 hours, preferably 8-12 hours.

[0028] Furthermore, in the above-mentioned method for preparing the silicon-aluminum material, as a specific implementation, the second silicon source in step (3) is one or more of water glass and alkaline silica sol, preferably alkaline silica sol.

[0029] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific embodiment, the acidic aluminum-containing compound in step (3) is a water-soluble acidic aluminum-containing compound, preferably a water-soluble acidic inorganic aluminum-containing compound, especially a water-soluble inorganic strong acid aluminum salt, more preferably selected from one or more of aluminum sulfate, aluminum nitrate, and aluminum chloride, preferably aluminum sulfate.

[0030] Furthermore, in the above-mentioned method for preparing silicon-aluminum materials, as a specific embodiment, the alkaline aluminum-containing compound in step (3) is an alkali metal aluminate solution; specifically selected from one or more of sodium aluminate and potassium aluminate, preferably sodium aluminate.

[0031] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific embodiment, the pH value of the mixed solution in step (3) is 4 to 7, preferably 5 to 6. The pH value of the mixed solution is regulated by the amount of the acidic aluminum-containing compound.

[0032] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the temperature in step (3) is 50°C to 90°C, preferably 50°C to 80°C.

[0033] Furthermore, in the above-mentioned preparation method of silicon-aluminum material, as a specific implementation mode, the aluminum content of the acidic aluminum-containing compound in step (3) is 10-70 gAl2O3 / L in terms of Al2O3, the aluminum content of the alkaline aluminum-containing compound is 70-170 gAl2O3 / L in terms of Al2O3, and the silicon content in the second silicon source is 20-80 gSiO2 / L in terms of SiO2.

[0034] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the amount of water used in step (3) is 10% to 20 vol%, preferably 13 to 20 vol%, of the total volume of the reaction system.

[0035] Furthermore, in the preparation method of the above-mentioned silicon-aluminum material, as a specific implementation, the second auxiliary agent in step (4) is a non-ionic surfactant, and the second auxiliary agent is one or more of polyethylene glycol, alkyl alcohol amide, and polyether; the alkyl alcohol amide is one or more of lauryl diethanolamine and coconut oil fatty acid diethanolamide; the polyether is one or more of AEO-6 and AEO-9; the molecular weight of the polyethylene glycol is 200 to 1000, preferably 200 to 700.

[0036] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the temperature in step (4) is 50°C to 90°C, preferably 50°C to 80°C.

[0037] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the mass ratio of the first material stream obtained in step (2) to the slurry in step (4) is 1:80-100.

[0038] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific embodiment, the hydrothermal treatment conditions in step (5) are: the treatment temperature is 100℃~180℃, preferably 110℃~160℃, and more preferably 120℃~150℃; the treatment pressure is 0.1~0.5MPa, preferably 0.1~0.3MPa, and the treatment time is 0.5h~10h, preferably 0.5h~6h.

[0039] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the washing in step (5) is washing with water, the washing temperature is 70-90° C., and the washing is performed several times, generally until the liquid becomes neutral.

[0040] Furthermore, in the above-mentioned method for preparing silicon-aluminum material, as a specific implementation, the drying conditions in step (5) are: drying temperature is 100-150° C., and drying time is 6-10 hours.

[0041] Furthermore, in the above-mentioned method for preparing the silicon-aluminum material, as a specific implementation, the calcination conditions in step (5) are: the calcination temperature is 500-700° C., and the calcination time is 4-8 hours.

[0042] Compared with the prior art, the silicon-aluminum material and its preparation method and application described in the present invention have the following advantages:

[0043] (1) The silicon-aluminum material provided by the present invention has a large pore volume and a two-level gradient pore channel of mesopore-macropore. The silicon-aluminum material has molecular sieve characteristics, and has the characteristics of high B acid content of molecular sieve and low impurity content (especially low sodium content). It is suitable for use as a catalytic material carrier, especially suitable for use as a carrier of heavy oil hydrogenation catalyst.

[0044] (2) In the method for preparing the silicon-aluminum material provided by the present invention, when preparing a semi-crystallized precursor, the over-crystallization of the precursor is regulated by adding a second auxiliary agent, and then the precursor is added to the silicon-aluminum material to allow the silicon-aluminum material to grow on its surface to form a high surface acidity and a mesoporous-macroporous ladder pore structure.

[0045] (3) In the method for preparing the silicon-aluminum material provided by the present invention, the precursor provides a crystal nucleus for the subsequent reaction, and the acidified silica gel group and aluminum hydroxide colloid are adsorbed on the crystal nucleus formed by the precursor, which promotes the increase of the grain size of the prepared silicon-aluminum material and is conducive to the formation of a silicon-aluminum material with a large pore volume, a large pore size and a strong acidity.

[0046] (4) In the method for preparing the silicon-aluminum material provided by the present invention, under preferred circumstances, by adding a second auxiliary agent, the soluble silicon species in the slurry is exchanged with the like ions on the surface of the second auxiliary agent micelles and adsorbed on the micelle surface, and also reacts with the second auxiliary agent molecules in the liquid phase to form a new inorganic-organic complex. The adsorbed silicon species micelles and composite molecules form a mesoporous material with a stable structure at a lower temperature through multiple thermodynamic equilibrium under the action of ionic bonds, hydrogen bonds and intermolecular dispersion forces. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is the XRD diagram of the silicon-aluminum material prepared in Example 1 of the present invention.

[0048] Figure 2 This is the nuclear magnetic resonance aluminum spectrum of the silicon-aluminum material prepared in Example 1 of the present invention.

[0049] Figure 3 This is the silicon nuclear magnetic resonance spectrum of the silicon aluminum material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0050] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings and specific embodiments. However, it should be pointed out that the protection scope of the present invention is not limited by these specific implementation modes, but is determined by the claims.

[0051] In the context of this specification, the pore volume, specific surface area and pore size distribution of the silicon-alumina material are measured by low-temperature nitrogen adsorption method. The total acid, B acid and L acid are measured by pyridine infrared adsorption method.

[0052] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.

[0053] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0054] Example 1

[0055] Prepare an aluminum sulfate solution with a concentration of 50gAl2O3 / L and a silica sol solution with a concentration of 60gSiO2 / L for later use.

[0056] Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 150gAl2O3 / L for later use.

[0057] 50 g of tetraethyl orthosilicate (TEOS), 70 g of tetrapropylammonium hydroxide (TPAOH), and 30 g of deionized water were mixed to form a sol, and then mixed with 15 g of glycerol and stirred and aged at 60° C. for 18 hours to obtain a precursor solution.

[0058] Add 500mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 65°C, add the prepared aluminum sulfate solution to the reactor at 16mL / min, and add the prepared sodium aluminate and silica sol in parallel, and control the pH of the reaction to 7.0 by adjusting the flow rate of sodium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum sulfate is 1320ml, the amount of sodium aluminate is 580mL, and the amount of silica sol is 1160ml. Add 20g of polyethylene glycol 200 to the reactor under stirring conditions, and then add 40g of the precursor solution to the above solution and stir until mixed evenly.

[0059] The slurry was placed in a reactor and treated at 100°C, 0.2 MPa and 8 hours under stirring. The treated slurry was washed with hot water at 90°C until the liquid was neutral, dried at 150°C for 6 hours to obtain dried sample AO-1, ​​and calcined at 600°C for 8 hours to obtain silicon-aluminum material A-1, the properties of which are shown in Table 1.

[0060] Example 2

[0061] Prepare an aluminum sulfate solution with a concentration of 60gAl2O3 / L and a silica sol solution with a concentration of 70gSiO2 / L for later use.

[0062] Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 140gAl2O3 / L for later use.

[0063] 50 g of tetraethyl orthosilicate (TEOS), 70 g of tetrapropylammonium hydroxide (TPAOH), and 30 g of deionized water were mixed to form a sol, and then mixed with 15 g of glycerol and stirred and aged at 60° C. for 18 hours to obtain a precursor solution.

[0064] Add 500mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 65°C, add the prepared aluminum sulfate solution to the reactor at 18mL / min, and add the prepared sodium aluminate and silica sol in parallel, and control the pH of the reaction to 6.5 by adjusting the flow rate of sodium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, 1300ml of aluminum sulfate, 600ml of sodium aluminate, and 1150ml of silica sol are added to the reactor under stirring conditions. 5g of polyethylene glycol 800 is then added to the reactor, and then 40g of the precursor solution is added to the above solution and stirred until mixed evenly.

[0065] The slurry was placed in a reactor and treated at 100°C, 0.1 MPa, and 8 hours under stirring. The treated slurry was washed with hot water at 90°C until the liquid was neutral, dried at 150°C for 6 hours to obtain dried sample AO-2, and calcined at 600°C for 8 hours to obtain silicon-aluminum material A-2, the properties of which are shown in Table 1.

[0066] Example 3

[0067] Prepare an aluminum chloride solution with a concentration of 30gAl2O3 / L and a water glass solution with a concentration of 30gSiO2 / L and a modulus of 2.5 for later use.

[0068] Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 100gAl2O3 / L for later use.

[0069] 60 g of methyl orthosilicate, 80 g of tetrapropylammonium hydroxide (TPAOH), and 40 g of deionized water were stirred to form a sol, and then mixed with 50 g of ethanol and aged at 80° C. for 8 hours to obtain a precursor solution.

[0070] Add 700mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 70°C, add the prepared aluminum chloride solution to the reactor at 14mL / min, and add the prepared sodium aluminate and water glass in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rate of sodium aluminate and water glass, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum chloride is 1100ml, the amount of sodium aluminate is 500mL, and the amount of water glass is 950ml. Add 10g of lauryl diethanolamine to the reactor under stirring conditions, and then add 45g of the precursor solution to the above solution and stir until mixed evenly.

[0071] The slurry was placed in a reactor and treated at 120°C, 0.2 MPa, and 4 hours under stirring. The treated slurry was washed with hot water at 70°C until the liquid was neutral, dried at 120°C for 8 hours to obtain dried sample AO-3, and calcined at 650°C for 6 hours to obtain silicon-aluminum material A-3, the properties of which are shown in Table 1.

[0072] Example 4

[0073] Prepare an aluminum chloride solution with a concentration of 10gAl2O3 / L and a water glass solution with a concentration of 20gSiO2 / L and a modulus of 2.5 for later use.

[0074] Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 70gAl2O3 / L for later use.

[0075] 60 g of methyl orthosilicate, 80 g of tetrapropylammonium hydroxide (TPAOH), and 40 g of deionized water were stirred to form a sol, and then mixed with 50 g of ethanol and aged at 80° C. for 8 hours to obtain a precursor solution.

[0076] Add 700mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, after the deionized water is heated to 70°C, add the prepared aluminum chloride solution to the reactor at 14mL / min, and add the prepared sodium aluminate and water glass in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rate of sodium aluminate and water glass, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum chloride is 1500ml, the amount of sodium aluminate is 500mL, and the amount of water glass is 1200ml. Add 5g of coconut oil fatty acid diethanolamide to the reactor under stirring conditions, and then add 45g of the precursor solution to the above solution, and stir until mixed.

[0077] The slurry was placed in a reactor and treated at a temperature of 120°C and a pressure of 0.2 MPa for 4 hours under stirring. The treated slurry was washed with hot water at 70°C until the liquid was neutral, dried at 120°C for 8 hours to obtain dried sample AO-4, and calcined at 650°C for 6 hours to obtain silicon-aluminum material A-4, the properties of which are shown in Table 1.

[0078] Example 5

[0079] Prepare an aluminum nitrate solution with a concentration of 70gAl2O3 / L and a silica sol solution with a concentration of 80gSiO2 / L for later use.

[0080] Prepare potassium aluminate solution with a caustic ratio of 1.20 and a concentration of 170gAl2O3 / L for later use.

[0081] 30 g of silica sol, 50 g of tetrapropylammonium hydroxide (TPAOH), and 20 g of deionized water were stirred to form a sol, and then mixed with 15 g of ethylene glycol and aged at 80° C. for 8 hours to obtain a precursor solution.

[0082] Add 1000mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 70°C, add the prepared aluminum nitrate solution to the reactor at 18mL / min, and add the prepared potassium aluminate and silica sol in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rates of potassium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum nitrate is 1500ml, the amount of potassium aluminate is 700mL, and the amount of silica sol is 1300ml. Add 10g AEO-9 to the reactor under stirring conditions, and then add 50g of the precursor solution to the above solution and stir until mixed evenly.

[0083] The slurry was placed in a reactor and treated at 180°C, 0.5 MPa, and 0.5 h under stirring. The treated slurry was washed with 80°C hot water until the liquid was neutral, dried at 100°C for 10 h to obtain dried sample AO-5, and calcined at 700°C for 4 h to obtain silicon-aluminum material A-5, the properties of which are shown in Table 1.

[0084] Example 6

[0085] Prepare an aluminum nitrate solution with a concentration of 40gAl2O3 / L and a silica sol solution with a concentration of 60gSiO2 / L for later use.

[0086] Prepare potassium aluminate solution with a caustic ratio of 1.20 and a concentration of 140gAl2O3 / L for later use.

[0087] 30 g of silica sol, 50 g of tetrapropylammonium hydroxide (TPAOH), and 20 g of deionized water were stirred to form a sol, and then mixed with 15 g of ethylene glycol and aged at 80° C. for 8 hours to obtain a precursor solution.

[0088] Add 1000mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 70°C, add the prepared aluminum nitrate solution to the reactor at 18mL / min, and add the prepared potassium aluminate and silica sol in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rates of potassium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum nitrate is 1600ml, the amount of potassium aluminate is 800mL, and the amount of silica sol is 1500ml. Add 10g AEO-6 to the reactor under stirring conditions, and then add 50g of the precursor solution to the above solution and stir until mixed evenly.

[0089] The slurry was placed in a reactor and treated at 180°C, 0.5 MPa, and 0.5 h under stirring. The treated slurry was washed with 80°C hot water until the liquid was neutral, dried at 100°C for 10 h to obtain dried sample AO-6, and calcined at 700°C for 4 h to obtain silicon-aluminum material A-6, the properties of which are shown in Table 1.

[0090] Comparative Example 1

[0091] Prepare an aluminum sulfate solution with a concentration of 50gAl2O3 / L and a silica sol solution with a concentration of 60gSiO2 / L for later use.

[0092] Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 150gAl2O3 / L for later use.

[0093] 50 g of tetraethyl orthosilicate (TEOS) and 30 g of deionized water were mixed to form a sol, and then mixed with 15 g of propylene glycol and stirred and aged at 60° C. for 18 hours to obtain a precursor solution.

[0094] Add 500mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 65°C, add the prepared aluminum sulfate solution to the reactor at 16mL / min, and add the prepared sodium aluminate and silica sol in parallel, and control the pH of the reaction to 7.0 by adjusting the flow rate of sodium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum sulfate is 1320ml, the amount of sodium aluminate is 580mL, and the amount of silica sol is 1160ml. Add 20g of polyethylene glycol 200 to the reactor under stirring conditions, and then add 40g of the precursor solution to the above solution and stir until mixed evenly.

[0095] The slurry was placed in a reactor and treated at 100°C, 0.2 MPa and 8 hours under stirring. The treated slurry was washed with hot water at 90°C until the liquid was neutral, dried at 150°C for 6 hours to obtain dried sample BO-1, and calcined at 600°C for 8 hours to obtain silicon-aluminum material B-1, the properties of which are shown in Table 1.

[0096] Comparative Example 2

[0097] Prepare an aluminum chloride solution with a concentration of 30gAl2O3 / L and a water glass solution with a concentration of 30gSiO2 / L and a modulus of 2.5 for later use.

[0098] Prepare a sodium aluminate solution with a caustic ratio of 1.20 and a concentration of 100gAl2O3 / L for later use.

[0099] 60 g of methyl orthosilicate, 80 g of tetrapropylammonium hydroxide (TPAOH), and 40 g of deionized water were stirred to form a sol, and then mixed with 50 g of ethanol and aged at 80° C. for 8 hours to obtain a precursor solution.

[0100] Add 700mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, after the deionized water is heated to 70°C, add the prepared aluminum chloride solution to the reactor at 14mL / min, and add the prepared sodium aluminate and water glass in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rate of sodium aluminate and water glass, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum chloride is 1100ml, the amount of sodium aluminate is 500mL, and the amount of water glass is 950ml, and then 45g of the precursor solution is added to the above solution and stirred until mixed evenly.

[0101] The slurry was placed in a reactor and treated at 120°C, 0.2 MPa, and 4 hours under stirring. The treated slurry was washed with hot water at 70°C until the liquid was neutral, dried at 120°C for 8 hours to obtain dried sample AO-3, and calcined at 650°C for 6 hours to obtain silicon-aluminum material A-3, the properties of which are shown in Table 1.

[0102] Comparative Example 3

[0103] Prepare an aluminum nitrate solution with a concentration of 70gAl2O3 / L and a silica sol solution with a concentration of 80gSiO2 / L and a modulus of 2.8 for later use.

[0104] Prepare potassium aluminate solution with a caustic ratio of 1.20 and a concentration of 170gAl2O3 / L for later use.

[0105] 30 g of silica sol and 20 g of deionized water were stirred to form a sol, and then mixed with 15 g of ethylene glycol and aged at 80° C. for 8 hours to obtain a precursor solution.

[0106] Add 1000mL of deionized water as bottom water to a 5000mL reactor, start stirring and heating, and after the deionized water is heated to 70°C, add the prepared aluminum nitrate solution to the reactor at 18mL / min, and add the prepared potassium aluminate and silica sol in parallel, and control the pH of the reaction to 6.0 by adjusting the flow rates of potassium aluminate and silica sol, and keep the slurry temperature and pH value in the reactor constant. After the reaction is completed, the amount of aluminum nitrate is 1500ml, the amount of potassium aluminate is 700mL, and the amount of silica sol is 1300ml, and then 50g of the precursor solution is added to the above solution and stirred until mixed evenly.

[0107] The slurry was placed in a reactor and treated at 180°C, 0.5 MPa, and 0.5 h under stirring. The treated slurry was washed with 80°C hot water until the liquid was neutral, dried at 100°C for 10 h to obtain the dried sample BO-3, and calcined at 700°C for 4 h to obtain the silicon-aluminum material B-3, the properties of which are shown in Table 1.

[0108] Table 1 Properties of Silicon Aluminum Materials

[0109] Sample name A-1 A-2 A-3 A-4 A-5 A-6 B-1 B-2 B-3 <![CDATA[Specific surface area, m 2 / g]]> 345 350 331 351 346 342 421 381 412 Pore ​​volume, mL / g 1.35 1.33 1.12 1.15 1.21 1.28 0.73 0.82 0.78 Average pore size, nm 21.1 20.2 18.1 17.8 18.3 19.8 6.9 8.6 7.6 Pore ​​size distribution, % <10nm 9.72 9.81 12.86 14.43 14.68 13.34 70.56 64.62 68.96 10-50nm 67.43 68.51 79.28 78.62 65.93 61.85 20.67 26.20 22.32 >50nm 22.85 21.68 7.86 6.95 19.39 22.81 8.77 9.18 8.72 B acid, mmol / g 0.231 0.220 0.196 0.184 0.187 0.182 0.105 0.126 0.103 B / L Ratio 1.19 1.09 0.92 0.95 0.89 0.84 0.42 0.52 0.36 <![CDATA[Na2O content, wt%]]> 0.28 0.31 0.38 0.34 0.19 0.21 0.45 0.24 0.19 <![CDATA[SiO2 content, wt%]]> 32.3 34.1 28.5 36.4 32.5 35.6 32.3 28.5 32.5

Claims

1. A silicon-aluminum material, which has the following properties after being calcined at 500-700°C: a silicon dioxide content of 20-40wt%, preferably 25-35wt%; a pore volume of not less than 0.70mL / g, preferably greater than 0.80mL / g, generally 0.70-1.5mL / g; a specific surface area of ​​280-400m 2 / g, preferably 300 to 400 m 2 / g.

2. The silicon-aluminum material according to claim 1, characterized in that: The calcined form of the silicon-aluminum material after calcination has an XRD pattern as shown in the following table; , The intensity value of the strongest diffraction peak in the XRD spectrum is defined as 100, then W represents weak, that is, relative intensity >0 to ≤20, M represents medium, that is, relative intensity >20 to ≤40, S represents strong, that is, relative intensity >40 to ≤60, and VS represents very strong, that is, relative intensity >60 to ≤100.

3. The silicon-aluminum material according to claim 1, characterized in that: In the nuclear magnetic resonance aluminum spectrum of the silicon-aluminum material, there are relatively strong absorption peaks near the chemical shifts of 59 ppm and 7 ppm.

4. The silicon-aluminum material according to claim 1, characterized in that: In the nuclear magnetic resonance silicon spectrum of the silicon-aluminum material, there is a strong absorption peak near the chemical shift of -88 ppm and a weak absorption peak at -111 ppm.

5. The silicon-aluminum material according to claim 1, characterized in that: The B acid content of the silicon-aluminum material is greater than 0.10 mmol / g, preferably 0.10 to 0.3 mmol / g, and more preferably 0.15 to 0.

35.

6. The silicon-aluminum material according to claim 1, characterized in that: The ratio of B acid to L acid in the silicon-aluminum material is 0.5 to 1.2, preferably 0.5 to 1.

0.

7. The silicon-aluminum material according to claim 1, characterized in that: The pore size distribution of the silicon-aluminum material has the following characteristics: the pore volume of pores with a pore diameter of less than 10 nm accounts for ≤15% of the total pore volume, the pore volume of pores with a pore diameter of 10-50 nm accounts for 50%-80% of the total pore volume, and the pore volume of pores with a pore diameter of >50 nm accounts for 5-35% of the total pore volume; preferably, the pore volume of pores with a pore diameter of less than 10 nm accounts for ≤10% of the total pore volume, the pore volume of pores with a pore diameter of 10-50 nm accounts for 60%-80% of the total pore volume, and the pore volume of pores with a pore diameter of >50 nm accounts for 10-30% of the total pore volume.

8. The silicon-aluminum material according to claim 1, characterized in that: The Na2O content of the silicon-aluminum material is less than 0.5wt%, preferably less than 0.3wt%.

9. A method for preparing a silicon-aluminum material, the preparation method comprising the following steps: (1) mixing a first silicon source, a first auxiliary agent and water under mixing conditions to obtain a sol; The first auxiliary agent is one or more of tetrapropylammonium hydroxide and tetrapropylammonium bromide; (2) mixing the sol obtained in step (1) with alcohol and then heat treating it to obtain a first stream; (3) adding a second silicon source, an acidic aluminum-containing compound, and an alkaline aluminum-containing compound into a reactor containing bottom water under contact conditions to obtain a mixed solution after reaction; (4) mixing the mixed solution obtained in step (3) with the second auxiliary agent under contact conditions to obtain a slurry; (5) Under contact conditions, the slurry obtained in step (4) and the first stream obtained in step (2) are mixed and hydrothermally treated, and after the treatment, the silicon-aluminum material is obtained by washing, drying and roasting.

10. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The first silicon source in step (1) is one or more of tetraethyl orthosilicate, methyl orthosilicate, and silica sol, preferably tetraethyl orthosilicate.

11. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The first auxiliary agent in step (1) is tetrapropylammonium hydroxide.

12. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The alcohol in step (2) is a C1-C3 alcohol.

13. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The alcohol in step (2) is one or more of ethanol, ethylene glycol, and glycerol, preferably glycerol.

14. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The mass ratio of the first silicon source, the first auxiliary agent, water and alcohol is 3-6:5-8:2-4:0.5-5.

15. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The heat treatment temperature in step (2) is 60 to 100° C., preferably 80 to 100° C.; the treatment time is no more than 24 hours, preferably 8 to 12 hours.

16. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The second silicon source in step (3) is one or more of water glass and alkaline silica sol, preferably alkaline silica sol.

17. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The acidic aluminum-containing compound in step (3) is a water-soluble acidic aluminum-containing compound, preferably a water-soluble acidic inorganic aluminum-containing compound, especially a water-soluble inorganic strong acid aluminum salt, more preferably one or more selected from aluminum sulfate, aluminum nitrate, and aluminum chloride, preferably aluminum sulfate.

18. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The alkaline aluminum-containing compound in step (3) is an alkali metal aluminate solution; selected from one or more of sodium aluminate and potassium aluminate, preferably sodium aluminate.

19. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The pH value of the mixed solution in step (3) is 4 to 7, preferably 5 to 6.

20. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The temperature in step (3) is 50°C to 90°C, preferably 50°C to 80°C.

21. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The aluminum content of the acidic aluminum-containing compound in step (3) is 10 to 70 gAl2O3 / L in terms of Al2O3, the aluminum content of the alkaline aluminum-containing compound is 70 to 170 gAl2O3 / L in terms of Al2O3, and the silicon content of the second silicon source is 20 to 80 gSiO2 / L in terms of SiO2.

22. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The amount of water used in step (3) is 10% to 20 vol%, preferably 13 to 20 vol%, of the total volume of the reaction system.

23. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The second auxiliary agent in step (4) is a nonionic surfactant, and the second auxiliary agent is one or more of polyethylene glycol, alkyl alcohol amide, and polyether; preferably polyethylene glycol.

24. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The pH value of the slurry in step (4) is 7.5 to 10.5, preferably 8.0 to 10.5, and more preferably 8.5 to 10.

5.

25. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The temperature in step (4) is 50°C to 90°C, preferably 50°C to 80°C.

26. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The mass ratio of the first material stream obtained in step (2) to the slurry in step (4) is 1:80-100.

27. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The hydrothermal treatment conditions in step (5) are as follows: the treatment temperature is 100°C to 180°C, preferably 110°C to 160°C, and more preferably 120°C to 150°C; the treatment pressure is 0.1 to 0.5 MPa, preferably 0.1 to 0.3 MPa; and the treatment time is 0.5h to 10h, preferably 0.5h to 6h.

28. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The washing in step (5) is performed with water at a washing temperature of 70 to 90°C.

29. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The drying conditions in step (5) are: drying temperature is 100-150° C., and drying time is 6-10 hours.

30. The method for preparing the silicon-aluminum material according to claim 9, characterized in that: The calcination conditions in step (5) are: calcination temperature is 500-700° C., and calcination time is 4-8 hours.

Citation Information

Patent Citations

  • High-activity silicon aluminum material and preparation method thereof

    CN108927208A

  • Porous silicon-aluminum material and preparation method thereof

    CN108927209A

  • Porous material and preparation method and application thereof

    CN111715202A

  • Silicon-aluminum particle aggregate as well as preparation method and application thereof

    CN114749170A

  • Mesostructured material with a high aluminium content

    US20090029847A1