Method for brazing Y2O3-MgO nano-composite ceramic and titanium alloy by adopting AgCu eutectic brazing filler metal
By brazing Y2O3-MgO nanocomplex ceramics and titanium alloys under vacuum conditions by AgCu eutectic brazing, the diffusion of Ti elements is used to form a strong interface combination, which solves the problem of low joint strength and airtightness, and achieves high strength and stability for infrared window materials.
Patent Information
- Application Number
- CN202411219967.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-26
AI Technical Summary
The connection between Y2O3-MgO nanocomposite ceramics and titanium alloys has problems such as low joint strength and airtightness and impermissible aging resistance, making it difficult to process and form complex components through traditional methods.
AgCu eutectic solder is used for brazing under vacuum. By melting the Ti element of the titanium alloy and diffusing with the Y2O3-MgO nano-complex ceramic side, a strong interface bond and continuous Ti-Cu interface reaction layer is formed to improve the joint. strength and stability.
It realizes high-strength and stable connection between Y2O3-MgO nanocomposite ceramics and titanium alloys, and the room temperature shear strength can reach 42MPa, which can maintain mechanical properties at high temperatures, and is suitable for the application of infrared window materials.
Smart Images

Figure CN119016821A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for brazing Y2O3-MgO nano composite ceramics and titanium alloy. Background Art
[0002] The infrared window is located at the front end of the infrared detector. It must ensure the efficient transmission of the target infrared radiation and protect the optical imaging detection system. It is an important structural / functional integrated component. Among the many infrared window materials, Y2O3-MgO nanocomposite ceramics have excellent infrared transmittance, low spontaneous radiation, excellent mechanical properties and thermal shock resistance, and have great application prospects in the application of infrared windows of high-speed aircraft in the future. In most cases, typical Y2O3-MgO nanocomposite ceramic components are usually complex in geometry and always need to be connected with other materials to form specific engineering components. However, due to the poor machinability and toughness of Y2O3-MgO nanocomposite ceramics and the lack of good processing properties like metal materials, it cannot be processed into complex-shaped components by traditional methods such as forging and extrusion molding. The production of large-sized and complex-shaped Y2O3-MgO nanocomposite ceramic components is very difficult, and they must be connected to themselves or to other materials through appropriate connection technology. Titanium alloys are widely used in the aerospace field due to their high specific strength, corrosion resistance, good high-temperature performance and excellent processing performance. If the Y2O3-MgO nanocomposite ceramics and titanium alloys can be reliably connected, the engineering applications of Y2O3-MgO nanocomposite ceramics can be broadened. Currently, mechanical connection and adhesive connection methods often have problems such as low joint strength, poor air tightness, and poor aging resistance. Summary of the invention
[0003] The present invention aims to solve the technical problems that the joints of Y2O3-MgO nanocomposite ceramics and metals obtained by the current mechanical method and adhesive bonding method have low strength and airtightness and are not resistant to aging, and provides a method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloys using AgCu eutectic solder.
[0004] The method of brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder of the present invention is carried out according to the following steps:
[0005] 1. Preparation of Y2O3-MgO nanocomposite ceramic matrix and titanium alloy matrix:
[0006] Cut the Y2O3-MgO nanocomposite ceramic matrix and the titanium alloy matrix, and then use 600#, 1000#, 2000# and 3000# metallographic sandpaper to grind the surfaces to be welded of the two matrixes until the surfaces are glossy, then put them into alcohol for ultrasonic cleaning for 10min to 15min, and blow dry them with a hair dryer for later use;
[0007] 2. Assembly of welding samples: Place the AgCu eutectic solder between the two base materials treated in step 1 to obtain a sandwich structure sample to be welded;
[0008] 3. Welding process: put the sandwich structure sample to be welded in step 2 into a vacuum furnace, place a graphite sheet on the upper end of the sample to be welded to apply a certain pressure to ensure that the sample surface is in close contact with the brazing filler metal during brazing, and evacuate; first raise the temperature from room temperature to 300℃~310℃, then raise the temperature to 730℃~790℃, then raise the temperature to 780℃~840℃ and keep it for 0~20min, then cool down to 300℃~320℃. The whole process is carried out under vacuum, and finally cool to room temperature with the furnace to complete the connection of Y2O3-MgO nanocomposite ceramics and titanium alloy by brazing using AgCu eutectic filler metal.
[0009] The beneficial effects of the present invention are as follows:
[0010] 1. The present invention uses a brazing method, which is easy to operate. AgCu eutectic brazing filler metal is used to successfully connect Y2O3-MgO nanocomposite ceramics and titanium alloy under vacuum conditions. Since the base material is titanium alloy, part of the Ti element can be dissolved into the liquid brazing filler metal after the brazing filler metal is melted, and wet bonding is achieved with one side of the Y2O3-MgO nanocomposite ceramics;
[0011] 2. The Ag-based solder in the present invention has excellent wettability to titanium alloy. During the brazing process, the Ti element melts from the surface of the titanium alloy base material into the liquid solder and diffuses to the Y2O3-MgO nanocomposite ceramic side. The active element Ti makes the solder also have excellent wettability to the Y2O3-MgO nanocomposite ceramic. The interfaces of the base materials on both sides are well bonded: the Ti element diffuses from the titanium alloy side to the Y2O3-MgO nanocomposite ceramic side and reacts with the MgO in the Y2O3-MgO to generate Ti3Cu3O oxide, and the Y2O3 phase is retained, thus forming a strong interface bond; at the same time, the solder reacts with the titanium alloy base material to generate a continuous Ti-Cu interface reaction layer; since the interface reaction of the base materials on both sides consumes a certain amount of Cu, the weld structure is mainly Ag-based solid solution, with a high melting point and plastic toughness;
[0012] 3. The present invention obtains a Y2O3-MgO nanocomposite ceramic / titanium alloy joint with excellent mechanical properties and capable of withstanding a certain high temperature. The room temperature shear strength of the joint obtained under the brazing process conditions of 800°C insulation for 0 min can reach 42 MPa. The present invention proposes a brazing method with high strength and stability in view of the current application status of the connection between infrared window material Y2O3-MgO nanocomposite ceramic and titanium alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is a backscattered electron scanning image of the joint obtained in Example 4;
[0014] Figure 2 for Figure 1 A partial enlarged view of the middle area A;
[0015] Figure 3 for Figure 2 Energy spectrum analysis diagram of phase 1 in the middle area;
[0016] Figure 4 for Figure 2 Energy spectrum analysis diagram of midpoint 2 phase;
[0017] Figure 5 for Figure 2 Energy spectrum analysis diagram of midpoint 3 phase;
[0018] Figure 6 for Figure 1 A partial enlarged view of the middle area B;
[0019] Figure 7 for Figure 6 Phase energy spectrum point analysis diagram of midpoint 4;
[0020] Figure 8 for Figure 6 Phase energy spectrum point analysis diagram of midpoint 5. DETAILED DESCRIPTION
[0021] Specific implementation method 1: This implementation method is a method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder, which is specifically carried out in the following steps:
[0022] 1. Preparation of Y2O3-MgO nanocomposite ceramic matrix and titanium alloy matrix:
[0023] Cut the Y2O3-MgO nanocomposite ceramic matrix and the titanium alloy matrix, and then use 600#, 1000#, 2000# and 3000# metallographic sandpaper to grind the surfaces to be welded of the two matrixes until the surfaces are glossy, then put them into alcohol for ultrasonic cleaning for 10min to 15min, and blow dry them with a hair dryer for later use;
[0024] 2. Assembly of welding samples: Place the AgCu eutectic solder between the two base materials treated in step 1 to obtain a sandwich structure sample to be welded;
[0025] 3. Welding process: put the sandwich structure sample to be welded in step 2 into a vacuum furnace, place a graphite sheet on the upper end of the sample to be welded to apply a certain pressure to ensure that the sample surface is in close contact with the brazing filler metal during brazing, and evacuate; first raise the temperature from room temperature to 300℃~310℃, then raise the temperature to 730℃~790℃, then raise the temperature to 780℃~840℃ and keep it for 0~20min, then cool down to 300℃~320℃. The whole process is carried out under vacuum, and finally cool to room temperature with the furnace to complete the connection of Y2O3-MgO nanocomposite ceramics and titanium alloy by brazing using AgCu eutectic filler metal.
[0026] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the Y2O3-MgO nanocomposite ceramic matrix described in step 1 is a dense ceramic material obtained by hot pressing or spark plasma sintering a mixture of nano Y2O3 powder and nano MgO powder in a volume ratio of 1:1. The rest is the same as specific embodiment 1.
[0027] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the titanium alloy base material described in step 1 is TC4 or TA15. The rest is the same as specific implementation method 1 or 2.
[0028] Specific implementation method 4: This implementation method is different from specific implementation methods 1 to 3 in that: in step 1, the sample is ultrasonically cleaned in alcohol for 12 minutes and dried with a hair dryer for later use. The rest is the same as specific implementation methods 1 to 3.
[0029] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that the AgCu eutectic solder described in step 2 is composed of 72% Ag and 28% Cu in terms of mass fraction. The rest is the same as specific embodiment 4.
[0030] Specific embodiment 6: This embodiment is different from specific embodiment 5 in that the AgCu eutectic solder described in step 2 is in the form of solder paste or foil. The rest is the same as specific embodiment 5.
[0031] Specific embodiment 7: This embodiment is different from specific embodiment 6 in that the AgCu eutectic solder paste described in step 2 is directly applied to the surface to be soldered. The rest is the same as specific embodiment 6.
[0032] Specific implementation eight: This implementation differs from specific implementation seven in that: the AgCu eutectic solder foil described in step two is cut to an area larger than the surface to be welded of the Y2O3-MgO nanocomposite ceramic, and then the two surfaces of the foil are polished with sandpaper to remove the surface impurity layer, and then ultrasonically cleaned in alcohol or acetone for 10 to 15 minutes, and blown dry for use. The rest is the same as specific implementation seven.
[0033] Specific embodiment 9: This embodiment differs from specific embodiment 8 in that: in step 3, the sandwich structure sample to be welded in step 2 is placed in a vacuum furnace, a graphite sheet is placed on the upper end of the sample to be welded to apply pressure to ensure that the sample surface is in close contact with the brazing material during brazing, and the vacuum is evacuated to a vacuum degree of 6×10 -3 The heating process starts as follows. The rest is the same as the eighth embodiment.
[0034] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that: in step 3, the temperature is first raised from room temperature to 300°C at a heating rate of 5°C / min, then raised to 730°C-790°C at a heating rate of 10°C / min, then raised to 780°C-840°C at a heating rate of 5°C / min and kept at that temperature for 0-20min, and then cooled to 300°C-320°C at a cooling rate of 5°C / min. The vacuum degree of the whole process is ≤1×10 -2 Pa, and finally cooled to room temperature in the furnace, and finally cooled to room temperature in the furnace to complete the connection of Y2O3-MgO nanocomposite ceramic and titanium alloy by brazing with AgCu eutectic brazing filler metal. The rest is the same as the ninth embodiment.
[0035] The present invention is verified by the following examples:
[0036] Embodiment: A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder is specifically carried out according to the following steps:
[0037] 1. Preparation of Y2O3-MgO nanocomposite ceramic matrix and titanium alloy matrix:
[0038] Cut the Y2O3-MgO nanocomposite ceramic matrix and the titanium alloy matrix, and then use 600#, 1000#, 2000# and 3000# metallographic sandpaper to grind the surfaces to be welded of the two matrixes until the surfaces are glossy, then put them into alcohol for ultrasonic cleaning for 12 minutes each, and blow dry them with a hair dryer for later use;
[0039] The Y2O3-MgO nanocomposite ceramic matrix is a dense ceramic material obtained by hot pressing and sintering a mixture of nano Y2O3 powder and nano MgO powder in a volume ratio of 1:1;
[0040] The titanium alloy base material is TC4;
[0041] 2. Assembly of welding samples: Place the AgCu eutectic solder between the two base materials treated in step 1 to obtain a sandwich structure sample to be welded;
[0042] The AgCu eutectic solder is a commercial product purchased, and its mass fraction composition is: 72% Ag and 28% Cu;
[0043] The AgCu eutectic solder is in the form of foil, which is cut to an area slightly larger than the surface to be welded of the Y2O3-MgO nanocomposite ceramic, and then the two surfaces of the foil are polished with sandpaper to remove the surface impurity layer, ultrasonically cleaned in alcohol for 12 minutes, and blown dry;
[0044] 3. Welding process: Place the sandwich structure sample to be welded in step 2 into a vacuum furnace. Place a graphite sheet on the upper end of the sample to be welded to apply a certain pressure to ensure that the sample surface is in close contact with the brazing material during brazing. Evacuate the furnace until the vacuum in the furnace is maintained at 6×10 -3 The heating procedure was then started; first, the temperature was raised from room temperature to 300°C at a heating rate of 5°C / min, then raised to 750°C at a heating rate of 10°C / min, then raised to 780°C-840°C at a heating rate of 5°C / min (see Table 1 for details) and kept at this temperature for 0-20min (see Table 1 for details), and then cooled to 300°C at a cooling rate of 5°C / min. The vacuum degree of the whole process was ≤1×10 -2 Pa, and finally cooled to room temperature in the furnace to complete the connection between Y2O3-MgO nanocomposite ceramics and titanium alloy by brazing with AgCu eutectic brazing filler metal.
[0045] According to the above process, a total of 6 groups of embodiments (embodiments 1-6) were carried out for comparison, corresponding to different brazing temperatures and holding times in the above step three, respectively. The other process parameters were the same, and the corresponding room temperature shear strength data of different joints were obtained, as shown in Table 1 below.
[0046] Table 1
[0047]
[0048] As can be seen from Table 1, when the welding method of the present invention is used to connect Y2O3-MgO nanocomposite ceramics and titanium alloy, the room temperature shear strength of the obtained joint can reach a maximum of 42 MPa (Example 6).
[0049] Figure 1 This is a backscattered electron scanning image of the joint obtained in Example 4. Region I is the Y2O3-MgO nanocomposite ceramic base material, region II is the weld, and region III is the TC4 titanium alloy base material. It can be seen that the joint is dense as a whole, and the interfaces on both sides are well bonded without obvious defects.
[0050] Figure 2 for Figure 1 A partial enlarged view of area A in the middle. Figure 3 , Figure 4 and Figure 5 They are Figure 2In the energy spectrum analysis diagram of the phases in region 1, point 2 and point 3, we can see the interlaced interface layers of the white Ag-based solid solution and the light gray Y2O3 on the Y2O3-MgO nanocomposite ceramic side, as well as a large number of dark gray Ti-Cu oxides and gray Ti-Cu compounds. The Ti element diffuses from the titanium alloy side to the Y2O3-MgO nanocomposite ceramic side and reacts with the MgO in the Y2O3-MgO to form Ti3Cu3O oxide, while the Y2O3 phase is retained ( Figure 3 ). Because the reaction product Ti3Cu3O is a brittle phase, and as the holding time increases, the reaction products become more and more, and will gradually move deeper into the weld, resulting in a decrease in joint strength; while as the holding time decreases, the reaction products also decrease, the interface reaction layer is thinner, the impact on the weld will also be reduced, and the mechanical properties will be stronger, which is consistent with the results in Table 1.
[0051] Figure 6 for Figure 1 A partial enlarged view of area B in the middle. Figure 7 and Figure 8 They are Figure 6 From the energy spectrum point analysis diagram of the phases at points 4 and 5, we can see the interface reaction layer between TC4 titanium alloy and the Ti-Cu compound of the solder.
[0052] Since the interface reaction of the base materials on both sides consumes a certain amount of Cu, the weld structure is mainly composed of Ag-based solid solution, which has a high melting point and plastic toughness.
Claims
1. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder, characterized in that The method of brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder is carried out according to the following steps:
1. Preparation of Y2O3-MgO nanocomposite ceramic matrix and titanium alloy matrix: Cut the Y2O3-MgO nanocomposite ceramic matrix and the titanium alloy matrix, and then use 600#, 1000#, 2000# and 3000# metallographic sandpaper to grind the surfaces to be welded of the two matrixes until the surfaces are glossy, then put them into alcohol for ultrasonic cleaning for 10min to 15min, and blow dry them with a hair dryer for later use; 2. Assembly of welding samples: Place the AgCu eutectic solder between the two base materials treated in step 1 to obtain a sandwich structure sample to be welded; 3. Welding process: put the sandwich structure sample to be welded in step 2 into a vacuum furnace, place a graphite sheet on the upper end of the sample to be welded to apply a certain pressure to ensure that the sample surface is in close contact with the brazing filler metal during brazing, and evacuate; first raise the temperature from room temperature to 300℃~310℃, then raise the temperature to 730℃~790℃, then raise the temperature to 780℃~840℃ and keep it for 0~20min, then cool down to 300℃~320℃. The whole process is carried out under vacuum, and finally cool to room temperature with the furnace to complete the connection of Y2O3-MgO nanocomposite ceramics and titanium alloy by brazing using AgCu eutectic filler metal.
2. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 1, characterized in that The Y2O3-MgO nanocomposite ceramic matrix described in step 1 is a dense ceramic material obtained by mixing nano Y2O3 powder and nano MgO powder in a volume ratio of 1:1 and then hot pressing or spark plasma sintering.
3. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 1, characterized in that The titanium alloy base material described in step 1 is TC4 or TA15.
4. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 1, characterized in that In step 1, place in alcohol and ultrasonically clean for 12 minutes, then blow dry with a hair dryer for later use.
5. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 1, characterized in that The AgCu eutectic solder described in step 2 is composed of 72% Ag and 28% Cu by mass.
6. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 5, characterized in that The AgCu eutectic solder described in step 2 is in the form of solder paste or foil.
7. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 6, characterized in that The AgCu eutectic solder paste described in step 2 is directly applied to the surface to be soldered.
8. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 6, characterized in that The AgCu eutectic solder foil described in step 2 is cut to an area larger than the surface to be welded of the Y2O3-MgO nanocomposite ceramic, and then both surfaces of the foil are polished with sandpaper to remove the surface impurity layer, ultrasonically cleaned in alcohol or acetone for 10 to 15 minutes, and blown dry for later use.
9. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 1, characterized in that In step 3, the sandwich structure sample to be welded in step 2 is placed in a vacuum furnace, and a graphite sheet is placed on the upper end of the sample to be welded to apply pressure to ensure that the sample surface is in close contact with the brazing material during the brazing process. The vacuum is evacuated until the vacuum degree is maintained at 6×10 -3 Start the heating process below.
10. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu eutectic solder according to claim 9, characterized in that In step 3, the temperature is first raised from room temperature to 300°C at a heating rate of 5°C / min, then raised to 730°C-790°C at a heating rate of 10°C / min, then raised to 780°C-840°C at a heating rate of 5°C / min and kept at that temperature for 0-20min, and then cooled to 300°C-320°C at a cooling rate of 5°C / min. The vacuum degree of the whole process is ≤1×10 -2 Pa, and finally cooled to room temperature with the furnace, and finally cooled to room temperature with the furnace to complete the connection of Y2O3-MgO nano-composite ceramics and titanium alloy brazing using AgCu eutectic brazing filler metal.
Citation Information
Patent Citations
Method for step-by-step brazing of magnesium fluoride ceramic and titanium alloy through metal and glass brazing filler metal
CN116532740A
Method for brazing zinc sulfide ceramic and titanium alloy through silver-based medium-temperature brazing filler metal
CN118060789A
Method for brazed connection of Y2O3-MgO nano-composite ceramic and titanium alloy
CN118492542A
Method for bonding members having different wettability with brazing material, its bonded body and its brazing material
JP1990248372A
Bonding method of ceramics with ti or ti alloy
JP1993286777A
Cited By
Method for assisting brazing of Y2O3-MgO nano-composite ceramic and titanium alloy by using plastic interlayer