Method for preparing TiAl-Co-based alloy based on high-energy ball milling and spark plasma sintering and preparation method of TiAl-Co-based alloy
By employing high-energy ball milling and spark plasma sintering, the problems of uneven composition and microstructure in TiAl-Co based alloys were solved, and TiAl-Co based alloys with good room temperature mechanical properties were prepared, which are suitable for hot-end components such as aero-engines.
Patent Information
- Application Number
- CN202411137099.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies make it difficult to prepare TiAl-Co based alloys with uniform microstructure and composition. Traditional smelting methods suffer from problems such as difficulty in controlling alloy composition, severe element segregation, and high smelting temperatures, resulting in poor alloy quality.
A TiAl-Co based alloy with fine grains and uniform composition was prepared by high-energy ball milling and spark plasma sintering.
The prepared alloy has good room temperature mechanical properties, dense structure and fine grains, and is suitable for practical applications in hot-end components such as aero-engines.
Smart Images

Figure CN119020628A_ABST
Abstract
Description
Technical Field
[0001] One or more embodiments of the present specification relate to the technical field of TiAl-Co based alloy powder metallurgy, and in particular, to a method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering and a preparation method thereof. Background Art
[0002] TiAl alloy has low density, high specific strength and specific stiffness, good comprehensive mechanical properties and anti-oxidation properties. It is an important material basis for the development of lightweight, high efficiency and long life of advanced aircraft engines. Almost all industrial countries in the world have invested a lot of energy in the fields of composition optimization and advanced preparation technology of the alloy. my country's aerospace medium and long-term development plan also has clear requirements for the development and application of the alloy. However, if TiAl alloy wants to compete with the widely used nickel-based high-temperature alloys and obtain practical applications in the hot end components of aircraft engines and gas turbines, it is urgent to make breakthroughs in the preparation and processing technology of high-quality alloys.
[0003] Studies have shown that γ-TiAl alloys with near-lamellar structures have high yield strength at room temperature, but low elongation, which does not meet the needs of aircraft engines. When the alloy has a dual-state structure, the plasticity is good, but the strength cannot meet the actual service requirements. Therefore, it is necessary to further adjust and optimize the organizational structure and composition of TiAl alloys. Co is a commonly used alloying element in high-temperature alloys. The strong β-stabilizing element Co can improve the electronic structure and elastic properties of TiAl alloys and improve the ductility of TiAl alloys. Adding a trace amount of rare earth element Y to refine and stabilize the alloy structure on the basis of Co alloying is expected to achieve a balance and comprehensive improvement between the toughness, plasticity, strength and creep resistance of the alloy.
[0004] An important factor that currently hinders the application of TiAl-Co based alloys is the difficulty in preparing and processing purified and homogenized alloys. Some traditional smelting methods have the disadvantages of being difficult to control the alloy composition, varying degrees of element segregation in the alloy, and high smelting temperatures, which lead to large shrinkage cavities in the alloy, making it difficult to prepare high-quality TiAl-Co based alloys. Compared with traditional smelting methods, TiAl-Co based alloys prepared by powder metallurgy have many special advantages, such as uniform and dense structure of the prepared alloy, fine grains, few defects such as shrinkage cavities and shrinkage, low temperature required for alloy preparation, and easy control of composition. Therefore, the powder metallurgy method has become an important means of preparing TiAl-Nb based multi-element alloys, and researchers at home and abroad have done a lot of work on this.
[0005] Powder metallurgy technology includes two processes: pre-alloy powder preparation and sintering. The particle size and uniformity of pre-alloy powder will affect the performance of sintered alloys. Common pre-alloy powder preparation methods include atomization, mechanical alloying (MA) and self-propagating high-temperature synthesis (SHS). The advantage of MA is that microcrystalline, nanocrystalline, supersaturated solid solution and amorphous pre-alloy powders can be prepared through high-energy ball milling. The prepared alloy composition is more uniform and a high energy storage powder system can be formed, which is conducive to reducing the temperature required for sintering and laying a good foundation for subsequent sintering alloys. The ball milling time has the greatest impact on the powder morphology during the MA process. Common sintering methods include spark plasma sintering (SPS), hot isostatic pressing (HIP) and hot pressing (HP). SPS pressurizes the powder and passes a high-frequency pulse current to activate the grain surface, break through the residual air in the pores, generate plasma through local discharge, and instantly generate local high temperature to achieve rapid sintering of the powder. SPS has the advantages of short sintering time, low temperature, dense sintered body and fine grains, and has become the most popular sintering method in recent years.
[0006] In summary, the present application now proposes a method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering and a preparation method thereof to solve the above-mentioned problems. Summary of the invention
[0007] The present invention aims to solve the problems raised in the background technology. The purpose of one or more embodiments of this specification is to propose a method for preparing a TiAl-Co based alloy based on high-energy ball milling and spark plasma sintering and a preparation method thereof. The alloy prepared by this method has fine grains, uniform composition, no segregation or little segregation, and good room temperature mechanical properties. The preparation method is simple and can effectively promote the practical engineering application of TiAl-Co based alloys.
[0008] Based on the above purpose, one or more embodiments of this specification provide a method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering, comprising the following steps:
[0009] S1, Ti powder, Al powder, Co powder and other powders are put into a ball mill according to a certain atomic percentage and mixed;
[0010] S2, adding a process control agent to the mixed powder and placing it in a vacuum glove box filled with high-purity argon gas;
[0011] S3, taking out the ball milling jar and placing it in a ball mill, setting the ball milling parameters and starting the ball milling, and after the ball milling is completed, placing the pre-alloyed powder in a vacuum glove box and then taking it out;
[0012] S4, loading the pre-alloyed powder into a graphite mold and setting the parameters of a spark plasma sintering machine to perform high-temperature spark plasma sintering, and finally obtaining a TiAl-Co based alloy.
[0013] The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in the embodiment of the present invention has fine grains, uniform composition, no segregation or little segregation, and good room temperature mechanical properties.
[0014] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the other powders in S1 are Nb powder and Y powder, the purity of the five elemental metal powders is greater than or equal to 99.95%, and the average particle size of the powder is 45 μm.
[0015] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the content of the powder in S1, i.e. the atomic percentage, is:
[0016] Al powder, 45-50%;
[0017] Co powder, 1-2%;
[0018] Nb powder, 5-8%;
[0019] Y powder, 0.1-0.5%;
[0020] The rest is Ti powder;
[0021] Among them, the total mass of the powder is 60g.
[0022] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the process control agent in S2 is n-hexane with a purity greater than 99.7% and an amount of 5-10% of the total mass of the powder.
[0023] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the ball mill in S3 is a planetary ball mill, the ball milling time is 20 to 25 hours, and the rotation speed is 400 to 500 rpm / min.
[0024] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the ball milling method in step S3 is an intermittent method, each ball milling takes 20 minutes, followed by a 10 minute break, and continues until the ball milling is completed.
[0025] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the pre-alloyed powder after high energy ball milling in S3 has been mechanically alloyed.
[0026] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, before loading the powder into the graphite grinding tool in S4, graphite foil needs to be pre-padded for separation.
[0027] According to the method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, in S4, before spark plasma sintering, the sintering furnace needs to be evacuated to a vacuum degree of 10 to 30 Pa; the sintering pressure is 20 to 50 MPa, and the sintering temperature is 1150 to 1250°C.
[0028] According to the method for preparing TiAl-Co based alloy based on high-energy ball milling and spark plasma sintering proposed in an embodiment of the present invention, the heating method for spark plasma sintering in S4 is to first heat the temperature to 570°C within 1S, then to 600°C within 6min, and finally to the target sintering temperature at a rate of 50-100°C / min, and the holding time is 6-12min; after the holding is completed, the pressure is maintained and the alloy is naturally cooled to room temperature with the furnace, and then the pressure is released and taken out.
[0029] According to the above, the present invention has the following beneficial effects:
[0030] The invention provides a method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering, which can overcome the problems of uneven structure and serious component segregation in the preparation of TiAl-Co based alloy in the prior art.
[0031] The present invention can complete mechanical alloying of single-element powders through high-energy ball milling, and can prepare pre-alloyed powders with fine particles and uniform internal structure. At the same time, through spark plasma sintering, an alloy with dense structure and fine grains can be prepared in a short time at a relatively low temperature. By controlling the temperature, TiAl-Co based alloys with different organizational morphologies can be obtained, showing good room temperature mechanical properties.
[0032] In summary, the present invention has the advantages of simple and efficient operation process, low raw material cost, strong repeatability, no need for complicated subsequent processing, and is suitable for industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate one or more embodiments of the present specification or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only one or more embodiments of the present specification. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 It is the microstructure morphology and cross-sectional morphology diagram of the mixed powder after ball milling for 20 hours;
[0035] Figure 2 This is a schematic diagram of the surface scanning results of the mixed powder after ball milling for 20 hours;
[0036] Figure 3 is the XRD pattern of the mixed powder after ball milling for 20 h;
[0037] Figure 4 Schematic diagram of the microstructure of the TiAl-Co alloy sintered at 1050° C. and 30 MPa in Example 1 of the present invention;
[0038] Figure 5 Schematic diagram of the microstructure of the TiAl-Co alloy sintered at 1150° C. and 30 MPa in Example 2 of the present invention;
[0039] Figure 6 This is a microstructure morphology diagram of the TiAl-Co alloy sintered at 1250° C. and 30 MPa in Example 3 of the present invention. DETAILED DESCRIPTION
[0040] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in conjunction with specific embodiments.
[0041] Example 1
[0042] (1) Mixing powder: 60 g of Ti powder, Al powder, Co powder, Nb powder and Y powder are prepared in the ratio of Ti-45Al-8Nb-1Co-0.3Y and put into a ball mill for mixing. The average particle size of the five metal powders is 45 μm and the purity is greater than 99.95%.
[0043] (2) Isolation from air: Add a process control agent to the mixed powder and place it in a vacuum glove box filled with high-purity argon gas. The process control agent is n-hexane with a purity greater than 99.7% and an amount of 8% of the total weight of the powder.
[0044] (3) High-energy ball milling: The ball mill is taken out and placed in a planetary ball mill. The ball milling time is 20 hours, the speed is set to 400 rpm / min, and the ball milling method is intermittent method. Each ball milling is 20 minutes, and the interval is 10 minutes. This is continued until the ball milling is completed. After the ball milling is completed, the ball mill is placed in a vacuum glove box and the powder is taken out. At this time, the powder has undergone mechanical alloying after a long period of high-energy ball milling.
[0045] (4) Preparation before sintering: Graphite foil is placed in the graphite mold in advance to prevent the alloy from sticking to the mold after sintering. The pre-alloyed powder is loaded into the graphite mold. The spark plasma sintering furnace is evacuated to a vacuum degree of 10 to 30 Pa in the furnace chamber.
[0046] (5) Sintering: After setting the sintering pressure to 30 MPa, the sintering temperature is increased to 570 °C within 1 second, then to 600 °C within 6 minutes, and then to 1050 °C at a rate of 50 °C / min. Then, the temperature and pressure are maintained at the set temperature and pressure for 10 minutes. After the insulation stage, the sample is cooled to room temperature with the furnace and the pressure is unloaded. When the pressure is released and the temperature is cooled to room temperature, the sample is demolded and taken out to obtain a Φ15 mm×5 mm TiAl-Co based alloy with high density, fine grains, uniform structure and good room temperature mechanical properties.
[0047] Example 2
[0048] (1) Mixing powder: 60 g of Ti powder, Al powder, Co powder, Nb powder and Y powder are prepared in the ratio of Ti-45Al-8Nb-1Co-0.3Y and put into a ball mill for mixing. The average particle size of the five metal powders is 45 μm and the purity is greater than 99.95%.
[0049] (2) Isolation from air: Add a process control agent to the mixed powder and place it in a vacuum glove box filled with high-purity argon gas. The process control agent is n-hexane with a purity greater than 99.7% and an amount of 8% of the total weight of the powder.
[0050] (3) Ball milling: The ball mill is taken out and placed in a planetary ball mill. The ball milling time is 20 hours, the speed is set to 400 rpm / min, and the ball milling method is intermittent method. Each ball milling is 20 minutes, and the interval is 10 minutes. This is continued until the ball milling is completed. After the ball milling is completed, the ball mill is placed in a vacuum glove box and the powder is taken out. At this time, the powder has undergone mechanical alloying after long-term high-energy ball milling;
[0051] (4) Preparation before sintering: Graphite foil is placed in the graphite mold in advance to prevent the alloy from sticking to the mold after sintering. The pre-alloyed powder is loaded into the graphite mold. The spark plasma sintering furnace is evacuated to a vacuum degree of 10 to 30 Pa in the furnace chamber.
[0052] (5) Sintering: After setting the sintering pressure to 30 MPa, the sintering temperature is increased to 570 °C within 1 second, then to 600 °C within 6 minutes, and then to 1150 °C at a rate of 50 °C / min. Then, the temperature and pressure are maintained at the set temperature and pressure for 10 minutes. After the insulation stage, the sample is cooled to room temperature with the furnace and the pressure is unloaded. When the pressure is released and the temperature is cooled to room temperature, the sample is demolded and taken out to obtain a Φ15 mm×5 mm TiAl-Co based alloy with high density, fine grains, uniform structure and good room temperature mechanical properties.
[0053] Example 3
[0054] (1) Mixing powder: 60 g of Ti powder, Al powder, Co powder, Nb powder and Y powder are prepared in the ratio of Ti-45Al-8Nb-1Co-0.3Y and put into a ball mill for mixing. The average particle size of the five metal powders is 45 μm and the purity is greater than 99.95%.
[0055] (2) Isolation from air: Add a process control agent to the mixed powder and place it in a vacuum glove box filled with high-purity argon gas. The process control agent is n-hexane with a purity greater than 99.7% and an amount of 8% of the total weight of the powder.
[0056] (3) Ball milling: The ball mill is taken out and placed in a planetary ball mill. The ball milling time is 20 hours, the speed is set to 400 rpm / min, and the ball milling method is intermittent method. Each ball milling is 20 minutes, and the interval is 10 minutes. This is continued until the ball milling is completed. After the ball milling is completed, the ball mill is placed in a vacuum glove box and the powder is taken out. At this time, the powder has undergone mechanical alloying after long-term high-energy ball milling;
[0057] (4) Preparation before sintering: Graphite foil is placed in the graphite mold in advance to prevent the alloy from sticking to the mold after sintering. The pre-alloyed powder is loaded into the graphite mold. The spark plasma sintering furnace is evacuated to a vacuum degree of 10 to 30 Pa in the furnace chamber.
[0058] (5) Sintering: After setting the sintering pressure to 30 MPa, the sintering temperature is increased to 570 °C within 1 second, then to 600 °C within 6 minutes, and then to 1250 °C at a rate of 50 °C / min. Then, the temperature and pressure are maintained at the set temperature and pressure for 10 minutes. After the insulation stage, the sample is cooled to room temperature with the furnace and the pressure is unloaded. When the pressure is released and the temperature is cooled to room temperature, the sample is demolded and taken out to obtain a Φ15 mm×5 mm TiAl-Co based alloy with high density, fine grains, uniform structure and good room temperature mechanical properties.
[0059] Comparative Example 1
[0060] (1) Mixing powder: 60 g of Ti powder, Al powder, Co powder, Nb powder and Y powder are prepared in the ratio of Ti-45Al-8Nb-1Co-0.3Y and put into a ball mill for mixing. The average particle size of the five metal powders is 45 μm and the purity is greater than 99.95%.
[0061] (2) Isolation from air: Add a process control agent to the mixed powder and place it in a vacuum glove box filled with high-purity argon gas. The process control agent is n-hexane with a purity greater than 99.7% and an amount of 8% of the total weight of the powder.
[0062] (3) Ball milling: The ball mill is taken out and placed in a planetary ball mill. The ball milling time is 20 hours, the speed is set to 400 rpm / min, and the ball milling method is intermittent method. Each ball milling is 20 minutes, and the interval is 10 minutes. This is continued until the ball milling is completed. After the ball milling is completed, the ball mill is placed in a vacuum glove box and the powder is taken out. At this time, the powder has undergone mechanical alloying after long-term high-energy ball milling;
[0063] (4) Preparation before sintering: Graphite foil is placed in the graphite mold in advance to prevent the alloy from sticking to the mold after sintering. The pre-alloyed powder is loaded into the graphite mold. The spark plasma sintering furnace is evacuated to a vacuum degree of 10 to 30 Pa in the furnace chamber.
[0064] (5) Sintering: After setting the sintering pressure to 30 MPa, the sintering temperature is increased to 570 °C within 1 second, then to 600 °C within 6 minutes, and then to 950 °C at a rate of 50 °C / min. Then, the temperature and pressure are maintained at the set temperature and pressure for 6 minutes. After the insulation stage, the sample is cooled to room temperature with the furnace and the pressure is unloaded. When the pressure is released and the temperature is cooled to room temperature, the sample is demolded and taken out. The porosity of the obtained TiAl-Co based alloy is significantly increased, the structure is uneven, and the room temperature mechanical properties are poor.
[0065] Comparative Example 2
[0066] (1) Mixing powder: 60 g of Ti powder, Al powder, Co powder, Nb powder and Y powder are prepared in the ratio of Ti-45Al-8Nb-1Co-0.3Y and put into a ball mill for mixing. The average particle size of the five metal powders is 45 μm and the purity is greater than 99.95%.
[0067] (2) Isolation from air: Add a process control agent to the mixed powder and place it in a vacuum glove box filled with high-purity argon gas. The process control agent is n-hexane with a purity greater than 99.7% and an amount of 8% of the total weight of the powder.
[0068] (3) Ball milling: The ball mill is taken out and placed in a planetary ball mill. The ball milling time is 20 hours, the speed is set to 400 rpm / min, and the ball milling method is intermittent method. Each ball milling is 20 minutes, and the interval is 10 minutes. This is continued until the ball milling is completed. After the ball milling is completed, the ball mill is placed in a vacuum glove box and the powder is taken out. At this time, the powder has undergone mechanical alloying after long-term high-energy ball milling;
[0069] (4) Preparation before sintering: Graphite foil is placed in the graphite mold in advance to prevent the alloy from sticking to the mold after sintering. The pre-alloyed powder is loaded into the graphite mold. The spark plasma sintering furnace is evacuated to a vacuum degree of 10 to 30 Pa in the furnace chamber.
[0070] (5) Sintering: After setting the sintering pressure to 30 MPa, the sintering temperature is raised to 570°C within 1 second, then raised to 600°C within 6 minutes, and then raised to 1350°C at a rate of 50°C / min. Then, the temperature and pressure are maintained at the set temperature and pressure for 10 minutes. After the insulation stage, the sample is cooled to room temperature with the furnace and the pressure is unloaded. When the pressure relief is completed and the temperature is cooled to room temperature, the sample is demolded and taken out. However, due to the high temperature, the mold is damaged, the obtained alloy is incomplete, and the mechanical properties are poor.
[0071] like Figure 1 As shown, the surface morphology and cross-sectional morphology of the powder after 20 hours of high-energy ball milling. It can be seen that at this time the powder has uniform and fine particle size, a high degree of spheroidization, and an evenly mixed internal structure with no obvious contrast in color.
[0072] like Figure 2 As shown, this is the EDS surface scanning distribution diagram of the powder cross-section morphology after 20 hours of high-energy ball milling. It can be seen that at this time, the elements inside the powder are basically mixed completely. The point scanning and selected area scanning analysis results also show that the internal composition of the powder at this time is close to the original powder composition ratio.
[0073] like Figure 3 As shown, this is the XRD spectrum of the powder after high-energy ball milling for 20 hours. It can be seen that at this time, the single peak has completely disappeared, indicating that the powder has completed mechanical alloying.
[0074] like Figure 4 As shown in Figure 3, it is the surface structure morphology of the alloy sintered by spark plasma sintering at 1050°C after the powder of mechanical alloying is completed. It can be seen that the alloy structure sintered at 1050°C is a near-γ structure, most of which is composed of equiaxed γ grains and a small amount of equiaxed α2 phases. At this time, the grains in the alloy structure are relatively small, and the average grain size is 2.53μm.
[0075] like Figure 5As shown in Figure 2, it is the surface structure morphology of the alloy sintered by spark plasma sintering at 1150°C after the powder of mechanical alloying is completed. It can be seen that the alloy sintered at 1150°C is a dual-state structure, mainly composed of equiaxed γ grains and α2+γ lamellae bundles, accompanied by the production of B2 precipitation phase. At this time, the average grain size reaches 4.31μm.
[0076] like Figure 6 As shown in Figure 2, it is the surface structure morphology of the alloy sintered by spark plasma sintering at 1250°C after the powder is mechanically alloyed. It can be seen that the volume content of α2+γ lamellar bundles in the alloy structure sintered at 1250°C is significantly increased, and the B2 precipitation phase increases. At this time, the microstructure of the alloy is near lamellar structure, and the average grain size reaches 5.26μm.
[0077] Product performance test:
[0078] The TiAl-Co based alloys obtained by the methods described in Examples 1 to 3 were subjected to density tests, room temperature hardness tests, and room temperature compression performance tests.
[0079] The difference between Comparative Example 1 and Examples 1 to 3 is that the sintering temperature is lower and the heat preservation and pressure holding time is shorter.
[0080] The difference between Comparative Example 2 and Examples 1 to 3 is that the sintering temperature is higher.
[0081] The results are shown in the following table:
[0082]
[0083] As can be seen from the above table, the titanium alloy treated by the method of the present invention is significantly better than the untreated titanium alloy substrate and the simple siliconized coating in terms of wear resistance and high temperature oxidation resistance. For the present invention, the comprehensive mechanical properties of Example 2 are the best.
[0084] In summary, friction and wear and high-temperature oxidation resistance experiments were carried out on the prepared composite gradient coating. The results show that the preparation method provided by the present invention has both excellent wear resistance and high-temperature oxidation resistance.
[0085] One or more embodiments of this specification are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of this specification should be included in the scope of protection of this disclosure.
Claims
1. A method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering, It is characterized in that The following steps are involved: S1, Ti powder, Al powder, Co powder and other powders are put into a ball mill according to a certain atomic percentage and mixed; S2, adding a process control agent to the mixed powder and placing it in a vacuum glove box filled with high-purity argon gas; S3, taking out the ball milling jar and placing it in a ball mill, setting the ball milling parameters and starting the ball milling, and after the ball milling is completed, placing the pre-alloyed powder in a vacuum glove box and then taking it out; S4, loading the pre-alloyed powder into a graphite mold and setting the parameters of a spark plasma sintering machine to perform high-temperature spark plasma sintering, and finally obtaining a TiAl-Co based alloy.
2. The method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that The other powders in S1 are Nb powder and Y powder. The purity of the five elemental metal powders is greater than or equal to 99.95%, and the average particle size of the powders is 45 μm.
3. The method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that The content (atomic percentage) of the powder in S1 is: Al powder, 45-50%; Co powder, 1-2%; Nb powder, 5-8%; Y powder, 0.1-0.5%; The rest is Ti powder; Among them, the total mass of the powder is 60g.
4. The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that The process control agent in S2 is n-hexane with a purity greater than 99.7% and an amount of 5-10% of the total mass of the powder.
5. The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that The ball mill in S3 is a planetary ball mill with a ball milling time of 20 to 25 hours and a rotation speed of 400 to 500 rpm / min.
6. The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that The ball milling method in step S3 is an intermittent method, with each ball milling for 20 minutes and an interval of 10 minutes, which is continued until the ball milling is completed.
7. The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that The pre-alloyed powder after high-energy ball milling in S3 has been mechanically alloyed.
8. The method for preparing TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that In the above-mentioned S4, before loading the powder into the graphite grinding tool, graphite foil needs to be pre-padded for separation.
9. The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that In the above S4, before spark plasma sintering, the sintering furnace needs to be evacuated to a vacuum degree of 10-30 Pa; the sintering pressure is 20-50 MPa, and the sintering temperature is 1150-1250°C.
10. The method for preparing a TiAl-Co based alloy based on high energy ball milling and spark plasma sintering according to claim 1, It is characterized in that In the S4, the temperature is first raised to 570°C within 1S, then raised to 600°C within 6min, and finally raised to the target sintering temperature at a rate of 50-100°C / min, and the holding time is 6-12min; After the heat preservation is completed, the pressure is maintained and the alloy is allowed to cool naturally to room temperature in the furnace before the pressure is released and taken out.