Ag-Cd diatomic electrocatalyst and preparation method and application thereof

The Ag-Cd diatomic electrocatalyst was synthesized by hydrothermal method, and the local coordination environment and strain environment were regulated, which solved the problems of low load and poor stability of the diatomic catalyst, achieved efficient CO2 reduction, significantly improved catalytic activity, and CO current was divided into two parts. Density and Faraday efficiency meet industrial requirements.

CN119020820APending Publication Date: 2024-11-26HUAIBEI NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110224.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing CO2 reduction electrocatalysts have low catalytic selectivity, poor stability and low current density, especially the low load of diatomic catalysts and difficult to control coordination environment, especially for carbon-based support, which leads to metal site migration during pyrolysis and Aggregation makes it difficult to regulate the coordination configuration of diatomic sites.

Method used

Ag-Cd diatomic electrocatalyst was synthesized by hydrothermal method, and Ag doping Cd3 (C3N3S3)2 was used to form AgN2S2-CdN2S2 diatomic sites, regulating the local coordination environment and strain environment, and avoiding metal migration and agglomeration during high-temperature carbonization , realize the controllable synthesis of diatom coordination structures.

Benefits of technology

The directional synthesis of high-load Ag-Cd diatomic sites was achieved, which improved CO2 reduction kinetics and significantly improved catalytic activity. The CO fraction current density can reach 200mA/cm-2, and the Faraday efficiency reached 99.9%, stability and selectivity Significant improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020820A_ABST
    Figure CN119020820A_ABST
Patent Text Reader

Abstract

The invention relates to an Ag-Cd diatomic electrocatalyst and a preparation method and application thereof. The preparation method comprises the following steps: preparation of a precursor Cd metal coordination polymer and preparation of an Ag-doped Cd coordination polymer: weighing Cd (NO3) 2.4 H2O, dispersing Cd (NO3) 2.4 H2O in deionized water, dissolving Cd (NO3) 2.4 H2O in deionized water to obtain a solution A, weighing Na3C3N3S3, dispersing Na3C3N3S3 in deionized water, and dissolving Na3C3N3S3 in deionized water to obtain a solution B; dropwise adding the solution B into the solution A, and sequentially stirring, centrifuging, washing, freezing and drying to obtain a Cd metal coordination polymer Cd3 (C3N3S3) 2; dispersing the Cd3 (C3N3S3) 2 and AgNO3 obtained in the previous step in deionized water, and stirring to obtain a mixed solution; carrying out hydrothermal reaction on the mixed solution, naturally cooling after the hydrothermal reaction is finished, and taking out a reacted sample; sequentially carrying out centrifugation, washing, freezing and drying on the sample to obtain Ag-doped Cd3 (C3N3S3) 2, and finally forming an AgN2S2-CdN2S2 diatomic site; according to the method, diatomic sites are effectively constructed through a proper method, the local matching and strain environment of active metal sites is adjusted, the adsorption of an intermediate is optimized, and the kinetics of CO2RR is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical catalysts, and in particular to an Ag-Cd diatomic electrocatalyst and a preparation method and application thereof. Background Art

[0002] The electrochemical CO2 reduction reaction (CO2RR) produces high-value chemicals and fuels. Among the many products, CO, as the core product of CO2 reduction, is the key raw material for Fischer-Tropsch synthesis and has a higher carbon fixation efficiency. Single-atom catalysts have been widely used in highly active CO production due to their atomic dispersion, clear active centers, adjustable coordination environment and maximum atomic utilization. However, CO2RR involves complex multi-step proton-electron transfer steps. Single-atom catalytic sites will have a high activation energy barrier when catalyzing CO2RR, thereby limiting the reaction kinetics. In order to overcome this technical problem, adjacent metal-modified single-atom sites are used to construct diatomic catalysts, which can effectively adjust the electronic state of single-atom catalysts and adjust their binding energy with different intermediates, thereby promoting the activation and conversion of CO2.

[0003] In order to study the synergistic effect and complementary functions of adjacent metal atoms, researchers have invested a lot of energy in the structural design and optimization of dual active sites. The coordination environment of diatomic sites can be optimized through strategies such as element type adjustment, atomic spacing regulation and coordination configuration optimization. For example, Lu Tongbu et al. used Te nanowires to connect ZIF-8 in series to prepare a core-shell structure, and synthesized a diatomic catalyst with TeN2-CuN3 sites after carbonization to promote the efficient reduction of CO2 [Nat. Commun. 2023, 14, 6164], Liu Bin [J. Am. Chem. Soc. 2023, 145, 11829-11836], Bu Xianhe [Adv. Mater. 2024, 36, 2309231] et al. synthesized Fe-Mo diatomic catalysts and sulfur-modified homonuclear Fe2 diatomic catalysts (Fe2N6-S) by impregnation method respectively; at the same time, strain engineering has also been proved to be an efficient strategy to improve the efficiency of CO2 by inducing changes in atomic spacing and symmetry. Changing the electronic structure of the catalytic site, for example, adjusting the atomic strain environment of the Fe-Ru diatomic site can control the electron occupancy of the antibonding orbital of the active Fe central atom, thereby adjusting the binding strength of the key reaction intermediates [Matter, 2024, 7, 1517–1532]; however, the loading of diatomic catalysts is usually less than 2wt%, which is relatively low, and the precise construction of the coordination environment is relatively difficult, especially for carbon-based supports. Due to thermodynamic instability and large surface energy, metal sites are prone to migration during pyrolysis, thereby agglomerating into metal clusters or particles, and it is difficult to adjust the coordination configuration of diatomic sites; therefore, in view of the low catalytic selectivity, poor stability and low current density of the developed CO2 reduction electrocatalysts, there is an urgent need for an Ag-Cd diatomic electrocatalyst and its preparation method and application, which can direct the synthesis of high-loaded Ag-Cd diatomic sites, solve the problems of difficult control of the coordination environment and low loading of conventional carbon-based diatomic catalysts, and thereby improve the CO2 reduction kinetics. Summary of the invention

[0004] The purpose of the present invention is to provide a Ag-Cd diatomic electrocatalyst and its preparation method and application, to effectively construct diatomic sites through a suitable method, to adjust the local coordination and strain environment of the active metal sites, to optimize the adsorption of intermediates, to promote the kinetics of CO2RR, and to solve the problems existing in the above-mentioned prior art.

[0005] A method for preparing an Ag-Cd diatomic electrocatalyst includes preparing a precursor Cd metal coordination polymer and preparing an Ag-doped Cd metal coordination polymer:

[0006] S1, Preparation of precursor Cd metal coordination polymer:

[0007] S1.1, weigh Cd(NO3)2·4H2O and disperse it in deionized water to dissolve to obtain solution A, weigh Na3C3N3S3 and disperse it in deionized water to dissolve to obtain solution B;

[0008] S1.2, drop solution B into solution A, stir, centrifuge, wash, freeze, and dry in sequence to obtain the precursor Cd metal coordination polymer Cd3(C3N3S3)2;

[0009] S2, Preparation of Ag-doped Cd metal coordination polymer:

[0010] S2.1, dispersing the Cd3(C3N3S3)2 and AgNO3 obtained in the above steps in deionized water, and stirring by ultrasonic to obtain a mixed solution;

[0011] S2.2, subjecting the mixed solution to a hydrothermal reaction, cooling it naturally after the hydrothermal reaction, and taking out the sample after the reaction;

[0012] S2.3, the above samples are centrifuged, washed, frozen and dried in sequence to obtain Ag-doped Cd metal coordination polymer Cd3(C3N3S3)2, and finally form AgN2S2-CdN2S2 diatomic sites.

[0013] Preferably, the mass ratio of Cd(NO3)2·4H2O and Na3C3N3S3 in S1.1 is 2-2.5:1-1.5; the mass volume ratio of Cd(NO3)2·4H2O and deionized water in solution A is 2-2.5 g:90-120 mL, and the mass volume ratio of Na3C3N3S3 and deionized water in solution B is 1-1.5 g:90-120 mL.

[0014] Preferably, the dropping rate of the Na3C3N3S3 solution in S1.2 is 190-210 mL / h, the stirring temperature is 24-25°C, the stirring time is 23-25 ​​hours, and the solution is washed with deionized water 2-4 times.

[0015] Preferably, the mass volume ratio of AgNO3 and deionized water in the mixed solution in S2.1 is 10 mg to 20 mg: 20 to 40 mL.

[0016] Preferably, the ultrasonic stirring time in S2.1 is 13 to 17 minutes.

[0017] Preferably, the mixed solution in S2.2 is transferred into a polytetrafluoroethylene liner, sealed and placed in a high-pressure reactor, and reacted in an oven at a temperature of 130° C. to 160° C. for 4 to 5 hours.

[0018] Preferably, in S2.3, the sample is washed 2 to 4 times in deionized water.

[0019] Preferably, the present invention discloses the preparation method for preparing Ag-Cd diatomic catalyst.

[0020] Preferably, the present invention discloses the use of the Ag-Cd diatomic catalyst in an electrocatalytic CO2 reduction reaction.

[0021] The present invention discloses the following technical effects:

[0022] 1. The present invention adopts a simple hydrothermal method to synthesize the Ag-Cd diatomic electrocatalyst, directionally constructs the AgN2S2-CdN2S2 diatomic sites, and the material morphology can be regulated by controlling the hydrothermal temperature. The process is simple and easy to control, and the raw materials are relatively cheap and easy to obtain. The diatomic sites prepared by the hydrothermal method avoid the conventional high-temperature carbonization process, and metal migration and agglomeration will not occur, thereby realizing the controllable synthesis of the diatomic coordination structure.

[0023] 2. The diatomic electrocatalyst prepared by the present invention is obtained by interstitially doping Ag into Cd3(C3N3S3)2. The introduction of Ag can regulate the local coordination environment of the Cd site to form local tensile strain. Compared with the pure Cd3(C3N3S3)2 catalyst, the microscopic morphology of Ag-doped Cd3(C3N3S3)2 changes significantly from an octahedron to an octahedron supported by a large number of nanorods, and the pore structure of the Ag-doped Cd3(C3N3S3)2 electrocatalyst is significantly enriched, with more active sites, which is conducive to the occurrence of electrocatalytic CO2 reduction and has good CO production performance.

[0024] 3. The enrichment of Cd electrons in the present invention is beneficial to the activation of CO2 and the adsorption of the key intermediate *COOH.

[0025] 4. The Ag-doped Cd3(C3N3S3)2 catalyst of the present invention has excellent catalytic activity in ionic liquid medium. In an H-type electrolytic cell, -2.3V vs.Ag / Ag + The Faradaic efficiency (FE) of electrocatalytic CO2 reduction to CO at the working potential of CO ) is the largest, which is 99.9%, and the CO current density can reach 150mA / cm –2 . In the wide range of working potentials from -2.5V to -2.1V, FE CO The CO current density can reach up to 200 mA / cm –2 , close to the level of industrial requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 : Schematic diagram of the synthesis of Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention;

[0028] Figure 2 : SEM image of Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention;

[0029] Figure 3 : SEM image of Ag-doped Cd3(C3N3S3)2-130 electrocatalyst prepared in Example 2 of the present invention;

[0030] Figure 4 : SEM spectrum of Ag-doped Cd3(C3N3S3)2-150 electrocatalyst prepared in Example 3 of the present invention;

[0031] Figure 5 : SEM spectrum of Ag-doped Cd3(C3N3S3)2-160 electrocatalyst prepared in Example 4 of the present invention;

[0032] Figure 6 : SEM spectrum of Cd3(C3N3S3)2-140 electrocatalyst prepared in Comparative Example 1 of the present invention;

[0033] Figure 7 : X-ray diffraction patterns of the Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention and the Cd3(C3N3S3)2-140 electrocatalyst prepared in Comparative Example 1;

[0034] Figure 8 : Energy dispersive X-ray spectroscopy (EDS) spectrum of the Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention;

[0035] Fig. 9 : High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image of the Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention;

[0036] Fig.10: R space curve and fitting curve diagram of K-edge Fourier transform extended X-ray absorption fine structure spectrum (FT-EXAFS) of Ag in Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention;

[0037] Fig.11 : R space curve and fitting curve diagram of K-edge FT-EXAFS of Cd in Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention;

[0038] Fig.12 : R space curve and fitting curve diagram of K-edge FT-EXAFS of Cd in Cd3(C3N3S3)2-140 electrocatalyst prepared in Comparative Example 1 of the present invention;

[0039] Fig.13 : CO2 reduction linear sweep voltammetry curves of the Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention and the Cd3(C3N3S3)2-140 prepared in Comparative Example 1;

[0040] Fig.14 : CO Faraday efficiency diagram of the Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1 of the present invention and the Cd3(C3N3S3)2-140 electrocatalyst prepared in Comparative Example 1 in ionic liquid electrolyte. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0043] Embodiment 1:

[0044] A method for preparing a Ag-Cd diatomic electrocatalyst, the method comprising the following steps:

[0045] (1) Preparation of precursor Cd metal coordination polymer: First, 2.31 g of cadmium nitrate tetrahydrate was ultrasonically dissolved in 100 mL of deionized water, recorded as solution A; then, 1.21 g of trisodium thiocyanate was ultrasonically dissolved in 100 mL of deionized water, recorded as solution B; subsequently, solution B was dripped into solution A at a rate of 200 mL / h, and finally ultrasonically stirred at 25°C for 24 hours, centrifuged to obtain a precipitate, washed three times with deionized water, and freeze-dried to obtain a yellow powder precursor Cd3(C3N3S3)2.

[0046] (2) Preparation of Ag-doped Cd metal coordination polymer: Weigh 0.1 g of precursor and 0.01 g of silver nitrate and dissolve them in 30 mL of deionized water. Ultrasonic stirring is performed for 15 min to obtain a mixed solution. The mixed solution is transferred into a polytetrafluoroethylene liner, sealed and placed in a high-pressure reactor. After reacting in an oven at 140°C for 5 hours, the product is taken out and collected by centrifugation. The product is washed three times with deionized water and finally freeze-dried to obtain Ag-doped Cd3(C3N3S3)2, thereby finally forming a diatomic site of AgN2S2-CdN2S2.

[0047] Example 2

[0048] The operating steps of Example 1 were repeated, except that the oven temperature was set to 130° C. to obtain an Ag-doped Cd metal coordination polymer.

[0049] Example 3

[0050] The operating steps of Example 1 were repeated, except that the oven temperature was set to 150° C. to obtain an Ag-doped Cd metal coordination polymer.

[0051] Example 4

[0052] The operating steps of Example 1 were repeated, except that the oven temperature was set to 160° C. to obtain an Ag-doped Cd metal coordination polymer.

[0053] Comparative Example 1

[0054] A method for preparing an electrocatalyst, the method comprising the following steps:

[0055] (1) Preparation of precursor Cd metal coordination polymer: First, 2.31 g of cadmium nitrate tetrahydrate was dissolved in 100 mL of deionized water, recorded as solution A; then, 1.21 g of trisodium thiocyanate was dissolved in 100 mL of deionized water, recorded as solution B; subsequently, solution B was dripped into solution A at a rate of 200 mL / h, and finally stirred at 25°C for 24 hours. The precipitate was washed three times with deionized water and freeze-dried to obtain a yellow powder precursor.

[0056] (2) Preparation of Cd metal coordination polymer without Ag doping: Weigh 0.1 g of the precursor and dissolve it in 30 mL of deionized water. Ultrasonic stirring is performed for 15 min to obtain a mixed solution. The mixed solution is transferred into a polytetrafluoroethylene liner, sealed and placed in a high-pressure reactor. After reacting in an oven at 140°C for 5 hours, the product is taken out and collected by centrifugation. It is washed three times with deionized water and finally freeze-dried to obtain the Cd metal coordination polymer without Ag doping.

[0057] Figure 1 Schematic diagram of the synthesis of the Ag-doped Cd3(C3N3S3)2-140 electrocatalyst prepared in Example 1; a precursor Cd metal coordination polymer is formed by coordination of metal Cd ions and trisodium thiocyanate (Na3C3N3S3), and then the Ag ions are anchored to the precursor by a 140-degree hydrothermal method to prepare an Ag-doped Cd coordination polymer having AgN2S2-CdN2S2 diatomic sites.

[0058] Figure 2-6 The scanning electron microscope images of Examples 1-4 and Comparative Example 1 are as follows; by observing the sample morphology, it is found that the morphology of Ag-doped and undoped Cd3(C3N3S3)2 coordination polymers changes significantly, the morphology of undoped Cd3(C3N3S3)2 is mainly a regular octahedron structure, and the surface of the regular octahedron is rough and porous, and after the introduction of Ag, it is found that irregularly shaped nanorods grow in situ on the surface of the regular octahedron, and as the hydrothermal temperature increases from 130°C to 160°C, the number of nanorods on the surface of the regular octahedron increases, and the morphology changes from rod-like to flake-like, indicating that the hydrothermal temperature can regulate the morphology of Ag-doped Cd3(C3N3S3)2, and appropriately increasing the temperature can effectively promote the growth of surface nanorods.

[0059] Figure 7 X-ray diffraction patterns of Ag-doped Cd3(C3N3S3)2 prepared by hydrothermal reaction at 140°C in Example 1 and Cd3(C3N3S3)2 prepared by hydrothermal reaction at 140°C in Comparative Example 1. It can be seen that the crystal structures of Ag-doped and undoped Cd3(C3N3S3)2 are similar, and no new substances appear. Compared with Cd3(C3N3S3)2 catalyst, the crystallization peak of Ag-doped Cd3(C3N3S3)2 shifts to a low angle, indicating that the overall interplanar spacing is significantly stretched, corresponding to the local tensile strain.

[0060] Figure 8 This is the EDS elemental energy spectrum of Ag-doped Cd3(C3N3S3)2 prepared in Example 1. It can be seen that S, C, N, Cd and Ag are evenly distributed, indicating that Ag is successfully and evenly dispersed in the Cd3(C3N3S3)2 coordination polymer without forming any metal particles.

[0061] Fig. 9 The HAADF-STEM image of Ag-doped Cd3(C3N3S3)2 prepared in Example 1 shows that Ag and Cd metals in Ag-doped Cd3(C3N3S3)2 are dispersed in the whole material in the form of atoms without metal agglomeration, which is consistent with the energy spectrum result.

[0062] Fig.10 The R space curve and fitting curve of the Ag K edge FT-EXAFS of the Ag doped Cd3(C3N3S3)2 electrocatalyst prepared in Example 12. As can be seen from the figure, the Ag K edge R space spectrum of Ag doped Cd3(C3N3S3)2 is An obvious scattering peak is shown at, corresponding to the scattering path of Ag-S. Through fitting, it can be seen that the first shell of Ag is coordinated with two S atoms, and the outer shell is coordinated with two N atoms and a small amount of Ag-Cd bonds. Finally, Ag is embedded in the Cd3(C3N3S3)2 coordination polymer in atomic form.

[0063] Fig.11 The R space curve and fitting curve of the Cd K edge FT-EXAFS of the Ag-doped Cd3(C3N3S3)2 electrocatalyst prepared in Example 1. It can be seen from the figure that the Cd K edge R space spectrum of Ag-doped Cd3(C3N3S3)2 is There is an obvious broad scattering peak at the scattering path corresponding to Cd-N / S. Through fitting, it can be seen that the first shell of Cd is coordinated with 2 S atoms and 2 N atoms. Combined with the EXAFS data of Ag atoms, it can be seen that the Ag-doped Cd3(C3N3S3)2 catalyst eventually forms a AgN2S2-CdN2S2 diatomic site (the inset is a schematic diagram of the AgN2S2-CdN2S2 atomic model).

[0064] Fig.12 The R space curve and fitting curve of the K-edge FT-EXAFS of Cd in the Cd3(C3N3S3)2 electrocatalyst prepared in Comparative Example 1; As can be seen from the figure, the R space spectrum of the Cd K-edge of Cd3(C3N3S3)2 is An obvious broad scattering peak is shown at, corresponding to the scattering path of Cd-N / S. Through fitting, it can be seen that the first shell of Cd is coordinated with 2 S atoms and 2 N atoms, and finally a CdN2S2 diatomic site is formed (illustration schematic diagram of CdN2S2 atomic model); compared with Cd3(C3N3S3)2, the Cd-S and Cd-N bond lengths in Ag-doped Cd3(C3N3S3)2 are increased, indicating that the Cd site will have local tensile strain after being doped with Ag atoms, which corresponds to the XRD results.

[0065] Fig.13 Linear scanning curve diagram of Ag-doped Cd3(C3N3S3)2 prepared in Example 2 and Cd3(C3N3S3)2 prepared in Comparative Example 1; it can be seen that the current density of Ag-doped Cd3(C3N3S3)2 in CO2-saturated electrolyte is significantly higher than that of Cd3(C3N3S3)2, proving that Ag-doped Cd3(C3N3S3)2 is more susceptible to CO2 reduction reaction during the linear scanning process.

[0066] Fig.14 The CO Faraday efficiency diagram of Ag-doped Cd3(C3N3S3)2 prepared in Example 1 and Cd3(C3N3S3)2 prepared in Comparative Example 1; it can be seen that the CO Faraday efficiency of Ag-doped Cd3(C3N3S3)2 is significantly higher than that of Cd3(C3N3S3)2, wherein, at the working potential of -2.3V, the maximum FE CO The CO current density can reach 150mA / cm –2 ; In particular, under a wide range of working potentials from -2.5V to -2.1V, FE CO The CO current density is higher than 99%, and the maximum current density of CO can reach about 200mA / cm –2 , close to the level of industrial requirements.

[0067] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a Ag-Cd diatomic electrocatalyst, characterized in that: Including the preparation of precursor Cd metal coordination polymer and the preparation of Ag-doped Cd metal coordination polymer; S1, Preparation of precursor Cd metal coordination polymer: S1.1, weigh Cd(NO3)2·4H2O and disperse it in deionized water to obtain solution A, weigh Na3C3N3S3 and disperse it in deionized water to obtain solution B; S1.2, drop solution B into solution A, stir, centrifuge, wash, freeze, and dry in sequence to obtain the precursor Cd metal coordination polymer Cd3(C3N3S3)2; S2, Preparation of Ag-doped Cd metal coordination polymer: S2.1, dispersing the Cd3(C3N3S3)2 and AgNO3 obtained in the above step in deionized water, and stirring to obtain a mixed solution; S2.2, subjecting the mixed solution to a hydrothermal reaction, cooling it naturally after the hydrothermal reaction, and taking out the sample after the reaction; S2.3, the above samples are centrifuged, washed, frozen and dried in sequence to obtain Ag-doped Cd metal coordination polymer Cd3(C3N3S3)2, and finally form AgN2S2-CdN2S2 diatomic sites.

2. The method for preparing a Ag-Cd diatomic electrocatalyst according to claim 1, characterized in that: The mass ratio of Cd(NO3)2·4H2O and Na3C3N3S3 in S1.1 is 2-2.5:1-1.5; the mass volume ratio of Cd(NO3)2·4H2O and deionized water in solution A is 2-2.5 g:90-120 mL, and the mass volume ratio of Na3C3N3S3 and deionized water in solution B is 1-1.5 g:90-120 mL.

3. The method for preparing a Ag-Cd diatomic electrocatalyst according to claim 1, characterized in that: The dropping rate of the Na3C3N3S3 solution in S1.2 is 190-210 mL / h, the stirring temperature is 24-25°C, the stirring time is 23-25 ​​hours, and the solution is washed with deionized water 2-4 times.

4. The method for preparing a Ag-Cd diatomic electrocatalyst according to claim 1, characterized in that: The mass volume ratio of AgNO3 and deionized water in the mixed solution in S2.1 is 10 mg to 20 mg: 20 to 40 mL.

5. The method for preparing a Ag-Cd diatomic electrocatalyst according to claim 1, characterized in that: The stirring time in S2.1 is 13 to 17 minutes.

6. The method for preparing a Ag-Cd diatomic electrocatalyst according to claim 1, characterized in that: The mixed solution in S2.2 is transferred into a polytetrafluoroethylene liner, sealed and placed into a high-pressure reactor, and reacted in an oven at a temperature of 130° C. to 160° C. for 4 to 5 hours.

7. The method for preparing a Ag-Cd diatomic electrocatalyst according to claim 1, characterized in that: The sample in S2.3 is washed 2 to 4 times in deionized water.

8. The Ag-Cd diatomic catalyst prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the Ag-Cd diatomic catalyst according to claim 8 in an electrocatalytic CO2 reduction reaction.