Preparation method of efficient defoaming agent and application of efficient defoaming agent in biochemical treatment of sewage
Preparation of refined polyether polyols by solid xylitol and mannitol, combining oxygen-containing solvents and emulsifiers, solves the problems of low efficiency and poor foam inhibition ability in wastewater biochemical treatment, and achieves rapid defoaming and long-term inhibition Bath, suitable for a variety of sewage treatments, and is microbial and environmentally friendly.
Patent Information
- Application Number
- CN202411321471.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-29
AI Technical Summary
In the biochemical treatment of sewage, existing defoamers have problems such as low defoaming efficiency, poor foam suppression ability, great impact on microorganisms, and environmental pollution. It is urgently needed to have a new defoamer that is efficient, low-cost and no impact.
Solid xylitol and solid mannitol are used as starting materials to prepare refined polyether polyols, combined with oxygen-containing solvents, emulsifiers and emulsification additives, and high-efficiency defoaming agents are prepared through emulsification treatment to reduce the surface tension of the foam and achieve rapid defoaming and Repress bubbles for a long time.
The prepared high-efficiency defoamer has the characteristics of fast defoaming, long-term foam suppression, microbial degradation, low dosage and good stability. It is suitable for a variety of sewage treatment systems and has no interference to biochemical treatment systems. It is suitable for large-scale production.
Smart Images

Figure BDA0005054069680000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biochemical sewage treatment, and in particular relates to a preparation method of a high-efficiency defoaming agent and application of the defoaming agent in biochemical sewage treatment. Background Art
[0002] A large amount of sewage is often generated in the process of household and industrial production. Sewage can only be safely discharged after being treated to meet the standards. Biochemical treatment is an important means to meet the standards of sewage treatment. It mainly uses the life metabolism of microorganisms to effectively remove soluble organic matter and some insoluble organic matter in sewage. However, since sewage contains organic matter such as carbohydrates, proteins, oils, lignin, etc., a large amount of foam is often generated during the aeration process, and the foam will continue to be generated, and even overflow from the biochemical pool, thereby causing pollution of external equipment and pool walls, worsening operating conditions, and even seriously affecting the biochemical treatment efficiency of sewage. The most effective, economical and simple way to solve the foaming problem in sewage biochemical treatment is to add a defoamer to the foaming system to quickly eliminate the foam and inhibit the generation of foam. Therefore, how to defoam and suppress foam has received widespread attention from all walks of life.
[0003] At present, defoamers can be divided into non-silicon type, polyether type, silicone type and silicone ether mixed type according to their composition. The main feature of non-silicon defoamers is low price, but poor ability to eliminate dense foam; polyether defoamers are non-toxic, odorless, well dispersed in water, and have strong anti-foaming ability, but low defoaming efficiency and cannot effectively eliminate a large amount of foam; silicone defoamers are widely used due to their many advantages such as high defoaming efficiency and good chemical stability, but their anti-foaming ability is poor, they will affect the development of mycelium, and silicon spots are not easy to remove, which are subject to certain restrictions in fermentation, sewage biochemical treatment, textile printing and dyeing and other industries. Due to the many shortcomings of existing defoamers, people are forced to study and find new and efficient defoamers for sewage biochemical treatment that have excellent defoaming and anti-foaming effects, no effect on microorganisms, no pollution to the environment, and low cost. Summary of the invention
[0004] In view of the above problems existing in the prior art, the present invention provides a method for preparing a high-efficiency defoaming agent and its application in the biochemical treatment of sewage. The high-efficiency defoaming agent of the present invention can be applied to a variety of sewage and biochemical treatment systems with large changes in water quality, can quickly reduce the surface tension of foam, has the characteristics of fast defoaming, strong foam suppression effect, small dosage, good stability, etc., can be degraded by microorganisms, has no interference with the biochemical treatment system, is suitable for large-scale production, and has good application prospects and market prospects.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The method for preparing a high-efficiency defoaming agent for biochemical treatment of sewage of the present invention comprises the following steps:
[0007] Step 1: Preparation of crude polyether polyols
[0008] Solid xylitol, solid mannitol and Fe-Zn double metal cyanide complex (DMC, commercially available) are put into a reactor, and the reaction is replaced with nitrogen three times and then vacuumed (gauge pressure ≤ -0.098MPa), and the temperature is raised to 110°C-130°C for vacuum dehydration for 1h, and then propylene oxide is added, and the pressure in the reactor is controlled to be maintained at 0.15-0.35MPa, and the temperature is raised to 130°C-150°C and stirred for 3h, and the temperature is lowered to room temperature after degassing; potassium hydroxide is added, and the temperature is raised to 110°C-130°C for vacuum dehydration for 3h, and then ethylene oxide is added, and the temperature is raised to 140°C-160°C and aged for 1h, and propyl gallate is added after the temperature is lowered to 90°C after degassing, and the mixture is stirred evenly to obtain a crude polyether polyol;
[0009] Step 2: Preparation of refined polyether polyols
[0010] The crude polyether polyol obtained in step 1 is heated to 70°C-80°C, 6.8-7.2% water is added, and the mixture is stirred for 0.5h, and the pH value of the reaction system is adjusted to 5.5-6.5 using a phosphoric acid solution. The mixture is stirred and mixed evenly, and then the mixture is heated to 90°C-100°C, and aluminum silicate is added for adsorption and decolorization. The mixture is filtered through a round mesh filter to obtain a refined polyether polyol.
[0011] Step 3: Preparation of high-efficiency defoaming agent for wastewater biochemical treatment
[0012] The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 60°C-75°C and stirred for 1 hour, and emulsified at a shearing speed of 3500-4500r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent for biochemical treatment of sewage.
[0013] The crude polyether polyol is prepared from the following raw materials in percentage by mass: 15-20% solid xylitol, 18-22% solid mannitol, 10-15% ethylene oxide, 40-50% propylene oxide, 0.003-0.008% Fe-Zn double metal cyanide complex, 0.2-0.3% potassium hydroxide, 0.05-0.1% propyl gallate, and the balance is water.
[0014] More preferably, the crude polyether polyol is made of the following raw materials in percentage by mass: 18% solid xylitol, 20% solid mannitol, 10% ethylene oxide, 45% propylene oxide, 0.006% Fe-Zn double metal cyanide complex, 0.25% potassium hydroxide, 0.08% propyl gallate, and the balance is water.
[0015] The high-efficiency defoamer for biochemical treatment of sewage comprises the following components by mass percentage: 55-65% of refined polyether polyol, 5-10% of oxygen-containing solvent, 10-20% of emulsifier, 1-2% of emulsifying aid, and the balance is water.
[0016] More preferably, the purified polyether polyol comprises 65%, the oxygen-containing solvent comprises 8%, the emulsifier comprises 15%, the emulsifying aid comprises 2%, and the balance is water.
[0017] The oxygen-containing solvent is composed of one or more of methanol, isopropanol and ethylene glycol. If there are more than one, the quality of each component is equal.
[0018] The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:1.
[0019] The emulsifying aid is composed of a mixture of one or more of hydrophobic silicon dioxide, hydroxypropyl methylcellulose and organic bentonite. If there are multiple components, the weight of each component is equal.
[0020] The stirring is carried out at a speed of 280-320 r / min.
[0021] The molar concentration of the phosphoric acid solution in step 2 is 0.3 mol / L; the amount of aluminum silicate used is 1.2-2.2% of the mass of the crude polyether polyol.
[0022] The high-efficiency defoaming agent for biochemical treatment of sewage can be applied to biochemical treatment systems with various sewage and large variations in water quality, and can be directly added and used in the sewage treatment process, with a dosage of 1 / 100,000 to 1 / 10,000 by volume.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention uses solid xylitol and solid mannitol as starting materials to prepare refined polyether polyols. The polyether polyols prepared from starting materials with low water content and high functionality can form an adsorption layer with better stability, which can enable the defoamer to better interact with the foam surface and effectively reduce its surface tension, thereby preventing the formation of foam and allowing the defoamer to have a long-lasting foaming effect. In addition, the added propyl gallate can reduce the odor of the refined polyether polyols caused by oxidative yellowing.
[0025] 2. The high-efficiency defoaming agent for biochemical treatment of sewage prepared by the present invention can be applied to biochemical treatment systems with various sewage and large changes in water quality. It only needs a small amount to achieve a good defoaming effect (the amount is one hundred thousandth to one ten thousandth, and it can be used directly in the sewage treatment process). It has excellent defoaming and foam suppression capabilities, and has rapid defoaming and long foam suppression time. It can be degraded by microorganisms, has no interference or impact on the biochemical treatment system, is suitable for large-scale production, and has good application prospects and market prospects. DETAILED DESCRIPTION
[0026] The above and other technical features and advantages of the present invention are described in more detail below.
[0027] Example 1: Formulation 1
[0028] The preparation method of the high-efficiency defoaming agent for biochemical treatment of sewage in this embodiment comprises the following steps:
[0029] Step 1: Preparation of crude polyether polyols
[0030] Solid xylitol, solid mannitol and Fe-Zn double metal cyanide complex were put into the reactor, and the atmosphere was replaced with nitrogen three times and then vacuumed (gauge pressure ≤ -0.098MPa). The temperature was raised to 120°C for vacuum dehydration for 1 hour, and then propylene oxide was added. The pressure in the reactor was controlled to be maintained at 0.2MPa. The temperature was raised to 140°C and stirred for 3 hours, and then the temperature was degassed and cooled to room temperature. Potassium hydroxide was added, and the temperature was raised to 120°C for vacuum dehydration for 3 hours, and then ethylene oxide was added. The temperature was raised to 150°C and aged for 1 hour. After degassing, propyl gallate was added when the temperature was lowered to 90°C, and the mixture was stirred evenly to obtain a crude polyether polyol.
[0031] Step 2: Preparation of refined polyether polyols
[0032] The crude polyether polyol obtained in step 1 is heated to 80° C., 7% water is added, and the mixture is stirred for 0.5 h. The pH of the reaction system is adjusted to 6.0 using a phosphoric acid solution. The mixture is stirred and mixed evenly, and then the mixture is heated to 100° C., and aluminum silicate is added for adsorption and decolorization. The mixture is filtered through a round mesh filter to obtain a refined polyether polyol.
[0033] Step 3: Preparation of high-efficiency defoaming agent for wastewater biochemical treatment
[0034] The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 70°C and stirred for 1 hour, and emulsified at a shearing speed of 4000r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent for biochemical treatment of sewage.
[0035] The crude polyether polyol is made of the following raw materials in percentage by mass: 18% solid xylitol, 20% solid mannitol, 10% ethylene oxide, 45% propylene oxide, 0.006% Fe-Zn double metal cyanide complex, 0.25% potassium hydroxide, 0.08% propyl gallate, and the balance is water. The high-efficiency defoamer for biochemical treatment of sewage includes the following components in percentage by mass: 65% refined polyether polyol, 8% oxygen-containing solvent, 15% emulsifier, 2% emulsifying aid, and the balance is water. The oxygen-containing solvent is composed of a mixture of isopropanol and ethylene glycol, and the mass of each component is equal. The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:1. The emulsifying aid is composed of hydroxypropyl methylcellulose and organic bentonite, and the mass of each component is equal.
[0036] Example 2: Formulation 2
[0037] The preparation method of the high-efficiency defoaming agent for biochemical treatment of sewage in this embodiment comprises the following steps:
[0038] Step 1: Preparation of crude polyether polyols
[0039] Solid xylitol, solid mannitol and Fe-Zn double metal cyanide complex were put into the reactor, and the atmosphere was replaced with nitrogen three times and then vacuumed (gauge pressure ≤ -0.098MPa). The temperature was raised to 110°C for vacuum dehydration for 1 hour, and then propylene oxide was added. The pressure in the reactor was controlled to be maintained at 0.15MPa. The temperature was raised to 130°C and stirred for 3 hours, and then the temperature was degassed and cooled to room temperature. Potassium hydroxide was added, and the temperature was raised to 110°C for vacuum dehydration for 3 hours, and then ethylene oxide was added. The temperature was raised to 145°C and aged for 1 hour. After degassing, propyl gallate was added when the temperature was lowered to 90°C, and the mixture was stirred evenly to obtain a crude polyether polyol.
[0040] Step 2: Preparation of refined polyether polyols
[0041] The crude polyether polyol obtained in step 1 is heated to 75° C., 7% water is added, and the mixture is stirred for 0.5 h, and the pH of the reaction system is adjusted to 6.0 using a phosphoric acid solution. The mixture is stirred and mixed evenly, and then the mixture is heated to 95° C., and aluminum silicate is added for adsorption and decolorization. The mixture is filtered through a round mesh filter to obtain a refined polyether polyol.
[0042] Step 3: Preparation of high-efficiency defoaming agent for wastewater biochemical treatment
[0043] The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 75°C and stirred for 1 hour, and emulsified at a shearing speed of 4000r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent for biochemical treatment of sewage.
[0044] The crude polyether polyol is made of the following raw materials in percentage by mass: 18% solid xylitol, 20% solid mannitol, 15% ethylene oxide, 40% propylene oxide, 0.008% Fe-Zn double metal cyanide complex, 0.3% potassium hydroxide, 0.05% propyl gallate, and the balance is water. The high-efficiency defoamer for biochemical treatment of sewage includes the following components in percentage by mass: 60% refined polyether polyol, 5% oxygen-containing solvent, 18% emulsifier, 1.5% emulsifying aid, and the balance is water. The oxygen-containing solvent is composed of a mixture of methanol and ethylene glycol, and the mass of each component is equal. The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:1. The emulsifying aid is composed of hydroxypropyl methylcellulose and hydrophobic silica, and the mass of each component is equal.
[0045] Example 3: Formulation 3
[0046] The preparation method of the high-efficiency defoaming agent for biochemical treatment of sewage in this embodiment comprises the following steps:
[0047] Step 1: Preparation of crude polyether polyols
[0048] Solid xylitol, solid mannitol and Fe-Zn double metal cyanide complex were put into the reactor, and the atmosphere was replaced with nitrogen three times and then vacuumed (gauge pressure ≤ -0.098MPa). The temperature was raised to 130℃ for vacuum dehydration for 1h, and then propylene oxide was added. The pressure in the reactor was controlled to be maintained at 0.3MPa. The temperature was raised to 145℃ and stirred for 3h, and then the temperature was degassed and cooled to room temperature. Potassium hydroxide was added, and the temperature was raised to 130℃ for vacuum dehydration for 3h, and then ethylene oxide was added. The temperature was raised to 160℃ and aged for 1h. After degassing, propyl gallate was added when the temperature was lowered to 90℃, and the mixture was stirred evenly to obtain a crude polyether polyol.
[0049] Step 2: Preparation of refined polyether polyols
[0050] The crude polyether polyol obtained in step 1 is heated to 80° C., 7% water is added, and the mixture is stirred for 0.5 h, and the pH value of the reaction system is adjusted to 6.5 using a phosphoric acid solution. The mixture is stirred and mixed evenly, and then the mixture is heated to 90° C., and aluminum silicate is added for adsorption and decolorization. The mixture is filtered through a round mesh filter to obtain a refined polyether polyol.
[0051] Step 3: Preparation of high-efficiency defoaming agent for wastewater biochemical treatment
[0052] The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 70°C and stirred for 1 hour, and emulsified at a shearing speed of 4500r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent for biochemical treatment of sewage.
[0053] The crude polyether polyol is made of the following raw materials in percentage by mass: 15% solid xylitol, 18% solid mannitol, 10% ethylene oxide, 50% propylene oxide, 0.004% Fe-Zn double metal cyanide complex, 0.2% potassium hydroxide, 0.1% propyl gallate, and the balance is water. The high-efficiency defoamer for biochemical treatment of sewage includes the following components in percentage by mass: 55% refined polyether polyol, 10% oxygen-containing solvent, 12% emulsifier, 1.8% emulsifying aid, and the balance is water. The oxygen-containing solvent is composed of a mixture of methanol, isopropanol and ethylene glycol, and the mass of each component is equal. The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:1. The emulsifying aid is composed of a mixture of hydrophobic silica, hydroxypropyl methylcellulose and organic bentonite, and the mass of each component is equal.
[0054] Comparative Example 1: Preparation 4
[0055] The preparation method of the high-efficiency defoaming agent for biochemical treatment of sewage in this embodiment comprises the following steps:
[0056] Step 1: Preparation of crude polyether polyols
[0057] Solid xylitol and Fe-Zn double metal cyanide complex were put into the reactor, and the atmosphere was replaced with nitrogen three times and then vacuumed (gauge pressure ≤ -0.098MPa). The temperature was raised to 120℃ and vacuum dehydrated for 1h, and then propylene oxide was added. The pressure in the reactor was controlled to be maintained at 0.2MPa. The temperature was raised to 140℃ and stirred for 3h, and then the temperature was degassed and cooled to room temperature. Potassium hydroxide was added, and the temperature was raised to 120℃ and vacuum dehydrated for 3h, and then ethylene oxide was added. The temperature was raised to 150℃ and aged for 1h. After degassing, propyl gallate was added when the temperature was lowered to 90℃, and stirred evenly to obtain crude polyether polyol.
[0058] Step 2: Preparation of refined polyether polyols
[0059] The crude polyether polyol obtained in step 1 is heated to 80° C., 7% water is added, and the mixture is stirred for 0.5 h. The pH of the reaction system is adjusted to 6.0 using a phosphoric acid solution. The mixture is stirred and mixed evenly, and then the mixture is heated to 100° C., and aluminum silicate is added for adsorption and decolorization. The mixture is filtered through a round mesh filter to obtain a refined polyether polyol.
[0060] Step 3: Preparation of high-efficiency defoaming agent for wastewater biochemical treatment
[0061] The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 70°C and stirred for 1 hour, and emulsified at a shearing speed of 4000r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent for biochemical treatment of sewage.
[0062] The crude polyether polyol is made of the following raw materials in percentage by mass: 38% solid xylitol, 10% ethylene oxide, 45% propylene oxide, 0.006% Fe-Zn double metal cyanide complex, 0.25% potassium hydroxide, 0.08% propyl gallate, and the balance is water. The high-efficiency defoamer for biochemical treatment of sewage includes the following components in percentage by mass: 65% refined polyether polyol, 8% oxygen-containing solvent, 15% emulsifier, 2% emulsifying aid, and the balance is water. The oxygen-containing solvent is composed of a mixture of isopropanol and ethylene glycol, and the mass of each component is equal. The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:1. The emulsifying aid is composed of hydroxypropyl methylcellulose and organic bentonite, and the mass of each component is equal.
[0063] Comparative Example 2: Preparation 5
[0064] The preparation method of the high-efficiency defoaming agent for biochemical treatment of sewage in this embodiment comprises the following steps:
[0065] Step 1: Preparation of crude polyether polyols
[0066] Solid mannitol and Fe-Zn double metal cyanide complex were put into the reactor, and the atmosphere was replaced with nitrogen three times and then vacuumed (gauge pressure ≤ -0.098MPa). The temperature was raised to 120°C for vacuum dehydration for 1 hour, and then propylene oxide was added. The pressure in the reactor was controlled to be maintained at 0.2MPa. The temperature was raised to 140°C and stirred for 3 hours, and then the temperature was degassed and cooled to room temperature. Potassium hydroxide was added, and the temperature was raised to 120°C for vacuum dehydration for 3 hours, and then ethylene oxide was added. The temperature was raised to 150°C and aged for 1 hour. After degassing, propyl gallate was added when the temperature was lowered to 90°C, and the mixture was stirred evenly to obtain a crude polyether polyol.
[0067] Step 2: Preparation of refined polyether polyols
[0068] The crude polyether polyol obtained in step 1 is heated to 80° C., 7% water is added, and the mixture is stirred for 0.5 h. The pH of the reaction system is adjusted to 6.0 using a phosphoric acid solution. The mixture is stirred and mixed evenly, and then the mixture is heated to 100° C., and aluminum silicate is added for adsorption and decolorization. The mixture is filtered through a round mesh filter to obtain a refined polyether polyol.
[0069] Step 3: Preparation of high-efficiency defoaming agent for wastewater biochemical treatment
[0070] The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 70°C and stirred for 1 hour, and emulsified at a shearing speed of 4000r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent for biochemical treatment of sewage.
[0071] The crude polyether polyol is made of the following raw materials in percentage by mass: 38% solid mannitol, 10% ethylene oxide, 45% propylene oxide, 0.006% Fe-Zn double metal cyanide complex, 0.25% potassium hydroxide, 0.08% propyl gallate, and the balance is water. The high-efficiency defoamer for biochemical treatment of sewage includes the following components in percentage by mass: 65% refined polyether polyol, 8% oxygen-containing solvent, 15% emulsifier, 2% emulsifying aid, and the balance is water. The oxygen-containing solvent is composed of a mixture of isopropanol and ethylene glycol, and the mass of each component is equal. The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:1. The emulsifying aid is composed of hydroxypropyl methylcellulose and organic bentonite, and the mass of each component is equal.
[0072] Example 4: Performance evaluation of high-efficiency defoaming agent for wastewater biochemical treatment
[0073] Thermal stability analysis: Take 5 g of each preparation sample, put it into a sealed test tube, and then place it in a 60°C oven for 48 hours. After taking it out, cool it to room temperature and observe whether the high-efficiency defoamer is separated into layers and floats into oil.
[0074] Centrifugal stability analysis: Take 8 mL of each preparation sample in a 10 mL centrifuge tube, set the centrifuge speed to 3000 r / min, and the centrifugation time to 30 min to observe whether the high-efficiency defoaming agent is separated into layers and floats into oil.
[0075] Compatibility analysis: Add 100 mL of aeration tank wastewater from the biochemical treatment system into a 250 mL beaker, add 1 mL of each preparation, stir magnetically for 10 minutes, and compare the precipitation of floating oil after standing for 1 hour.
[0076] Evaluation method of defoaming performance: add 50 mL of aeration tank sewage in the biochemical treatment system into a 250 mL measuring cylinder, add 0.05 g of each preparation respectively, and blow nitrogen into the foaming liquid through a glass tube at a flow rate of 500 mL / min. When the foam height exceeds the 250 mL scale, stop blowing nitrogen and pull out the glass tube. At the same time, start recording the time required for the foam to drop from 250 mL to 50 mL scale, which is the defoaming time. Test 3 times and take the average value as the final result.
[0077] Evaluation method for antifoaming performance: add 50 mL of aeration tank sewage in the biochemical treatment system into a 250 mL measuring cylinder, add 0.05 g of each preparation respectively, and blow nitrogen into the foaming liquid through a glass tube at a flow rate of 500 mL / min. At the same time, start recording the time required for the foam to rise from 50 mL to 250 mL, which is the antifoaming time. Test 3 times and take the average value as the final result.
[0078] Sewage biochemical treatment experiment: Measure 500mL of biochemical liquid into a beaker, put the aeration head into the biochemical liquid to start aeration, and continue aeration for 1 day. Add 1 / 100,000 of preparations 1, 2, 3 and commercially available conventional defoaming agents. Use no defoaming agent as a blank control, test the COD and TN values of the biochemical liquid before and after the experiment, and calculate the COD and TN removal rates.
[0079] The experimental results show that: as shown in Table 1, compared with conventional defoamers on the market, the high-efficiency defoamer for biochemical treatment of sewage prepared in the embodiment has better stability and compatibility, and its defoaming performance and foam inhibition performance are better, among which the defoaming effect and foam inhibition effect of preparation 1 are the best; compared with the COD and TN removal rates of the blank control (no defoamer added) (the blank sample COD removal rate is 78.68%, and the TN removal rate is 67.78%), the addition of the defoamer of the embodiment preparation has no significant interference with the COD and TN removal rates in the biochemical treatment system.
[0080] According to the comparison between preparations 1, 2, 3 and preparations 4, 5 in Table 1, it can be obtained that the defoaming time of the high-efficiency defoamer for biochemical treatment of sewage prepared with solid xylitol and solid mannitol (preparations 1, 2, 3) is shorter than that of the high-efficiency defoamer prepared with single use (preparations 4, 5), and the foam suppression time is longer than that of the high-efficiency defoamer prepared with single use (preparations 4, 5), indicating that the defoaming performance and foam suppression performance of the high-efficiency defoamer for biochemical treatment prepared with solid xylitol or solid mannitol as a single starting material are lower than those of the high-efficiency defoamer for biochemical treatment prepared with solid xylitol and solid mannitol as starting materials.
[0081] Table 1 Performance evaluation test results of different preparations
[0082]
[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a high-efficiency defoamer, characterized in that The steps include: Step 1: Preparation of crude polyether polyols Solid xylitol, solid mannitol and Fe-Zn double metal cyanide complex are put into a reaction kettle, evacuated after nitrogen replacement, heated to 110-130°C for vacuum dehydration, and then propylene oxide is added, the pressure in the reaction kettle is controlled to be maintained at 0.15-0.35MPa, heated to 130-150°C and stirred for 3h, and then cooled to room temperature after degassing; potassium hydroxide is added, heated to 110-130°C for vacuum dehydration, and then ethylene oxide is added, heated to 140-160°C for aging, and after degassing, propyl gallate is added when the temperature drops to 90°C, and stirred evenly to obtain a crude polyether polyol; Step 2: Preparation of refined polyether polyols The crude polyether polyol prepared in step 1 is heated to 70°C-80°C, water is added, stirred for 0.5h, the pH value of the reaction system is adjusted, stirred and mixed evenly, heated to 90°C-100°C, aluminum silicate is added for adsorption and decolorization, and filtered to obtain a refined polyether polyol; Step 3: Preparation of high-efficiency defoaming agent The refined polyether polyol, oxygen-containing solvent and emulsifier obtained in step 2 are heated to 60°C-75°C and stirred for 1 hour, and emulsified at a shearing speed of 3500-4500r / min for 20 minutes using a shear emulsifier. The emulsifying aid and water are slowly added under stirring, and the stirring is continued for 1 hour before discharging the material to obtain a high-efficiency defoaming agent.
2. The preparation method according to claim 1, characterized in that: In step 1, the crude polyether polyol is prepared from the following raw materials in percentage by mass: 15-20% solid xylitol, 18-22% solid mannitol, 10-15% ethylene oxide, 40-50% propylene oxide, 0.003-0.008% Fe-Zn double metal cyanide complex, 0.2-0.3% potassium hydroxide, 0.05-0.1% propyl gallate, and the balance is water.
3. The preparation method according to claim 2, characterized in that: In step 1, the crude polyether polyol is prepared from the following raw materials in percentage by mass: 18% solid xylitol, 20% solid mannitol, 10% ethylene oxide, 45% propylene oxide, 0.006% Fe-Zn double metal cyanide complex, 0.25% potassium hydroxide, 0.08% propyl gallate, and the balance is water.
4. The preparation method according to claim 1, characterized in that: In step 2, a phosphoric acid solution is used to adjust the pH of the reaction system to 5.5-6.
5.
5. The preparation method according to claim 1, characterized in that: In step 3, the raw materials of the high-efficiency defoamer include the following components by mass percentage: 55-65% of refined polyether polyol, 5-10% of oxygen-containing solvent, 10-20% of emulsifier, 1-2% of emulsifying aid, and the balance is water.
6. The preparation method according to claim 5, characterized in that: In step 3, the raw materials of the high-efficiency defoamer include the following components by mass percentage: 65% of refined polyether polyol, 8% of oxygen-containing solvent, 15% of emulsifier, 2% of emulsifying aid, and the balance of water.
7. The preparation method according to claim 5, characterized in that: The oxygen-containing solvent is composed of one or more of methanol, isopropanol and ethylene glycol. If there are more than one, the quality of each component is equal.
8. The preparation method according to claim 5, characterized in that: The emulsifier is composed of nonylphenol polyoxyethylene ether and dehydrated mannitol fatty acid ester polyoxyethylene ether, and the mass ratio of each component is 1:
1.
9. The preparation method according to claim 5, characterized in that: The emulsifying aid is composed of a mixture of one or more of hydrophobic silicon dioxide, hydroxypropyl methylcellulose and organic bentonite. If there are multiple components, the weight of each component is equal.
10. Use of the high-efficiency defoamer prepared by the preparation method according to any one of claims 1 to 9 in biochemical treatment of sewage, characterized in that: The high-efficiency defoaming agent is directly added and used in the sewage treatment process, and the dosage is 1 / 100,000 to 1 / 10,000 of the sewage by volume.
Citation Information
Patent Citations
Preparation method of defoaming agent for fermenting polymer
CN113440893A
Composite polyether defoaming agent for fermentation and preparation method thereof
CN117402346A
Special low-odor environment-friendly anti-rust oil for automobile parts and preparation method thereof
CN117586822A
Defoaming agent special for biochemical treatment as well as preparation method and application thereof
CN117839278A
Process for preparing reactive polyether polyols having an ethylene oxide end block
CN1946765A