Preparation method and application of high-flux anti-scaling loose nanofiltration membrane
Through the inorganic salt anion regulation interface polymerization reaction, the diffusion rate of small molecule polyamine is controlled, and the problem of insufficient selective permeability and anti-scaling performance of polyamide thin film composite nanofiltration membrane is solved, and high-throughput, anti-scaling and anti-scaling are prepared Loosen the nanofiltration membrane, improving water treatment efficiency and membrane service life.
Patent Information
- Application Number
- CN202411342456.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-29
AI Technical Summary
Polyamide film composite nanofiltration membrane has shortcomings in selective permeability and anti-scattering properties, resulting in low membrane flux and prone to scaling, affecting water treatment efficiency and cost.
The interfacial polymerization reaction is regulated by inorganic salt anion, and the electrostatic interaction between anions and small-molecular polyamines is used to control the diffusion rate of small-molecular polyamines, adjust the thickness and pore size of the membrane, and improve the separation performance and anti-scattering performance of the membrane.
A high-throughput, scaling-resistant loose nanofiltration membrane is prepared, which improves water treatment efficiency and membrane service life, while reducing treatment costs and wastewater discharge.
Smart Images

Figure CN119034513A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, relates to performance improvement of a nanofiltration membrane used in sewage treatment, and specifically relates to a method for improving the flux and anti-scaling performance of a nanofiltration membrane. Background Art
[0002] With the rapid development of society and economy, people are paying more and more attention to organic micropollutants (such as antibiotics) in water. These pollutants are usually present in very low concentrations in water, but they can cause serious harm to human health and the ecological environment. The physical and chemical properties of organic micropollutants are relatively complex, and it is difficult to completely remove them with conventional physical, chemical and biological treatment technologies. Membrane separation has high separation efficiency and low separation cost, and has gradually become a physical separation method for efficient removal of organic micropollutants.
[0003] As a membrane separation technology, polyamide thin film composite nanofiltration membrane can selectively remove micropollutants and high-valent ions, showing unique selective separation characteristics, and is widely used in the treatment of organic pollutants. At present, there are two problems with polyamide thin film composite nanofiltration membrane: one is that there is a selective permeability trade-off line for nanofiltration membranes, and the selective permeability cannot be further improved; the other is that the membrane surface is easy to scale during operation, especially under high recovery conditions. The first problem is caused by the characteristics of the interfacial polymerization reaction itself: the interfacial polymerization reaction is a self-terminating reaction, and the thickness of the polyamide membrane cannot be adjusted, resulting in a low membrane flux; the interfacial polymerization reaction is too fast, and the interface is unstable, resulting in excessive free volume in the membrane. The second problem is crucial to improving the efficiency of surface water and groundwater treatment. The concentration of ions and pollutants in surface water and groundwater is usually low, and it is necessary to reduce the treatment cost and improve the water utilization rate by increasing the recovery rate. In this process, the membrane surface is very easy to scale, which affects the service life of the membrane.
[0004] By regulating the physical and chemical microstructure of the nanofiltration membrane, improving the separation and transmission conditions of the membrane and the charge on the membrane surface, not only the separation performance of the membrane can be improved, but also the anti-scaling performance under high recovery conditions can be improved. This is of great significance in reducing water treatment costs, improving treatment efficiency, reducing wastewater discharge and increasing membrane service life. Summary of the invention
[0005] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing a high-flux anti-fouling loose nanofiltration membrane, by regulating the interfacial polymerization reaction by inorganic salt anions, and controlling the diffusion rate of the small molecule polyamine by utilizing the electrostatic interaction between the anions and the small molecule polyamine. The interfacial polymerization reaction regulated by anions can not only reduce the thickness of the nanofiltration membrane and adjust the pore size of the nanofiltration membrane, but also increase the density and electronegativity of the carboxyl groups on the membrane surface, selectively remove micropollutants while ensuring high flux, and at the same time have certain anti-fouling performance.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0007] One aspect of the present invention provides a method for preparing a high-flux anti-fouling loose nanofiltration membrane, comprising the following steps:
[0008] S1. Add an inorganic salt solution to the aqueous polyamine solution and adjust the pH value to 10 to 11.5 to obtain an interfacial polymerization aqueous solution;
[0009] S2. The ultrafiltration base membrane for the experiment is fully infiltrated with the interfacial polymerization aqueous solution, and then dried in the air until there is no obvious water stain on the membrane surface, thereby obtaining an ultrafiltration base membrane fully infiltrated with the aqueous solution;
[0010] S3. pouring the oil phase solution (i.e., the polyacyl chloride solution) onto the surface of the aqueous ultrafiltration substrate membrane, so that the polyacyl chloride solution is fully in contact with the aqueous polyamine monomer, and a polymerization reaction occurs fully, thereby forming a layer of polyamide ultrathin film on the aqueous ultrafiltration substrate membrane; the polyacyl chloride solution includes polyacyl chlorides and an organic solvent;
[0011] S4. The prepared polyamide membrane is annealed to obtain a high-flux anti-fouling loose nanofiltration membrane.
[0012] Interfacial polymerization is divided into an aqueous phase and an oil phase. In the present invention, the aqueous phase is a mixed aqueous solution composed of polyamines and inorganic salts, and the oil phase is polyacyl chlorides dissolved in an organic solvent. The electrostatic interaction between inorganic anions and polyamines is used to regulate the diffusion rate of the polyamines, thereby preparing a high-throughput, anti-scaling loose nanofiltration membrane.
[0013] Preferably, in step S1, the inorganic salt is selected from one or more of a fluoride salt system, a bromide salt system, a nitrate system, a silicate system, a tungstate system, a molybdate system, a permanganate system, a sulfate system, a sulfite system and a pyrophosphate system; and the concentration of the inorganic salt in the interfacial polymerization aqueous phase solution is 0.01 to 0.5 M.
[0014] Preferably, in step S1, the polyamine solution is prepared by adding a polyamine monomer into water, and the polyamine monomer is selected from at least one of piperazine, m-phenylenediamine, p-phenylenediamine, melamine, thiourea, polyethyleneimine, diethyltriamine and N-aminoethylpiperazine.
[0015] Preferably, in step S2, the ultrafiltration base membrane material is selected from any one of polysulfone, polyethersulfone, polyvinylidene fluoride, polyacrylonitrile, polytetrafluoroethylene nylon, cellulose or a cellulose derivative; and the pore size of the ultrafiltration base membrane is 0.01 to 2 μm.
[0016] Preferably, in step S3, the organic solvent is selected from at least one of hexane, heptane, pentane, Isopar G, toluene, ethyl acetate and benzene.
[0017] Preferably, in step S3, the polyacyl chloride is selected from at least one of 1,3,5-trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, azelaic acid chloride, adipic acid chloride, and 2,2',4,4'-biphenyltetracarboxylic acid chloride; and the concentration of the polyacyl chloride in the polyacyl chloride solution is 0.25-7.5 mg / ml.
[0018] Preferably, in step S3, the polyamine monomer and the polyacyl chloride are subjected to an interfacial polymerization reaction at an interface temperature of 20 to 35° C. and a relative humidity of 50 to 100% for 30 to 90 seconds.
[0019] Preferably, in step S4, the annealing treatment is performed at a temperature of 20 to 80° C. and for a time of 1 to 30 minutes.
[0020] Another aspect of the present invention provides a high-flux anti-fouling loose nanofiltration membrane, which is prepared by the above preparation method. The separation layer of the high-flux anti-fouling loose nanofiltration membrane (i.e., the polyamide ultra-thin film prepared in step S3) has a thickness of 8 to 230 nm and a smooth structure; the molecular weight cutoff MWCO of the high-flux anti-fouling loose nanofiltration membrane reaches 350 to 500 Da, and the pore radius of the separation layer reaches 0.45 to 0.55 nm; the carboxyl density of the high-flux anti-fouling loose nanofiltration membrane reaches 0.8 to 1.5 sites·nm -3 ;
[0021] The pure water flux of the high-flux anti-scaling loose nanofiltration membrane is 40 L·h -1 ·m -2 bar -1 As mentioned above, the retention rates of tetracycline and norfloxacin reached over 96%; the retention rate of PEG600 reached over 96%; under the premise of ensuring high retention rate of specific substances, the water flux and anti-scaling performance were improved.
[0022] Another aspect of the present invention provides the use of the high-flux anti-scaling loose nanofiltration membrane in water treatment, and the high-flux anti-scaling loose nanofiltration membrane is applied to sewage treatment.
[0023] The above technical solution has at least the following beneficial effects:
[0024] 1. The present invention provides a method for improving the flux and anti-fouling performance of a nanofiltration membrane, through which a high-flux, anti-fouling nanofiltration membrane can be obtained.
[0025] 2. The present invention combines the nanofiltration membrane structure and the interfacial polymerization reaction control method, designs and optimizes the diffusion rate of small molecule amines, and uses the electrostatic interaction between anions and small molecule polyamines to control the diffusion rate of small molecule polyamines. The electrostatic force is a long-range force with a larger range of action and a stronger force. It can greatly reduce the diffusion rate of small molecule polyamines, thereby affecting the interfacial polymerization reaction, thereby preparing a high-throughput anti-fouling loose nanofiltration membrane.
[0026] 3. The preparation method of the present invention reduces the thickness of the separation layer of the nanofiltration membrane by regulating the diffusion rate of the polyamine, appropriately increases the carboxyl density and pore size of the nanofiltration membrane, and improves the water flux and anti-scaling performance of the nanofiltration membrane while ensuring the retention rate of antibiotic pollutants.
[0027] 4. The preparation method of the present invention solves the problems of the traditional method being complicated, high cost and unsatisfactory effect. The preparation method is simple, low cost, has obvious and stable regulation effect, is convenient for large-scale preparation, and has strong industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 : SEM image of the surface of the high-throughput anti-fouling loose nanofiltration membrane prepared in Example 1.
[0029] Figure 2 : SEM image of the surface of the conventional nanofiltration membrane prepared in Comparative Example 1. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present invention, in order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention, and preferred embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood. The present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited to the specific embodiments disclosed below.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0032] Polyamide nanofiltration membrane is prepared by interfacial polymerization of trimesoyl chloride and small molecule amine at the oil-water interface. First, the small molecule amine in the aqueous phase diffuses into the oil phase, and secondly, the acyl chloride group crosses the interface to react chemically with the amino group in the aqueous phase. The intrinsic reaction rate of interfacial polymerization is high, and too fast a reaction affects the uniformity and thickness of the polyamide membrane, resulting in the inability to further improve the membrane performance. Therefore, by adjusting the diffusion rate of the small molecule amine, the reaction rate-controlling step, the reaction rate of the polymerization reaction can be regulated.
[0033] In view of the deficiencies in the prior art, the inventors of this case unexpectedly discovered through research and practice that the electrostatic interaction between anions and small molecule amines is a long-range force with a larger range of action and a stronger force, which can control the diffusion rate of small molecule amines to a large extent, thereby affecting the interfacial polymerization reaction. Based on this discovery, the technical solution of the present invention is proposed, that is, while ensuring the high performance of the nanofiltration membrane, the flux of the nanofiltration membrane is improved, and the risk of scaling of the nanofiltration membrane is reduced, and a method for preparing a high-throughput anti-scaling loose nanofiltration membrane is provided, as well as the application of the nanofiltration membrane prepared by the method in water treatment. The technical solution, its implementation process, etc. will be explained as follows.
[0034] The present invention provides a method for preparing a high-flux anti-scaling loose nanofiltration membrane, comprising the following steps:
[0035] 1) adding a polyamine monomer into water to obtain a polyamine solution;
[0036] The polyamine monomer is selected from at least one of piperazine, m-phenylenediamine, p-phenylenediamine, melamine, thiourea, polyethyleneimine, diethyltriamine and N-aminoethylpiperazine.
[0037] 2) Adding an inorganic salt solution to the aqueous polyamine solution, adjusting the pH value to 10-11.5, to obtain an interfacial polymerization aqueous solution; the pH of the interfacial polymerization aqueous solution will affect the flux and selectivity of the final product membrane, and needs to be controlled at 10-11.5. If the pH is too high, the polymerization reaction will be too intense, which will easily lead to a decrease in membrane flux. If the pH is too low, the selectivity of the membrane for inorganic salts, pollutants, etc. will be affected;
[0038] The inorganic salt is selected from one or more of a fluoride salt system, a bromide salt system, a nitrate system, a silicate system, a tungstate system, a molybdate system, a permanganate system, a sulfate system, a sulfite system and a pyrophosphate system;
[0039] The inorganic salt concentration in the interfacial polymerization aqueous phase solution is 0.001-0.5 M. If the concentration is too high, the inorganic salt will form crystals during the preparation process, affecting the integrity of the membrane. If the concentration is too low, the regulating effect on the polymerization reaction is weak.
[0040] 3) using the interfacial polymerization aqueous solution to fully infiltrate the ultrafiltration base membrane for the experiment for 10 to 120 seconds, and then drying it in the air until there is no obvious water stain on the membrane surface, thereby obtaining an ultrafiltration base membrane fully infiltrated with the aqueous solution;
[0041] The ultrafiltration base membrane material is selected from any one of polysulfone, polyethersulfone, polyvinylidene fluoride, polyacrylonitrile, polytetrafluoroethylene nylon, cellulose or cellulose derivatives; the pore size of the ultrafiltration base membrane is 0.01-2 μm, and its pore size strongly affects the interfacial polymerization reaction, and the pore size determines the amount of aqueous solution in the pore size. Specifically, the pore size affects the interfacial polymerization reaction on the one hand. The base membrane pore size is small, the aqueous solution content is high, and the interfacial polymerization reaction is complete. The base membrane pore size is large, the aqueous solution is relatively small, and the interfacial polymerization reaction is relatively incomplete; on the other hand, the pore size affects the effective membrane area (the small pore size means the small effective water area after water passes through the separation layer), thereby affecting the membrane permeability.
[0042] 4) using a polyacyl chloride solution to fully infiltrate the surface of the aqueous ultrafiltration substrate membrane, allowing the polyamine monomer and the polyacyl chloride to undergo interfacial polymerization reaction at an interface temperature of 20 to 35° C. and a relative humidity of 50 to 100% for 30 to 90 seconds, thereby forming a polyamide ultrathin separation layer on the surface (front) of the aqueous ultrafiltration substrate membrane, and then performing annealing treatment at a temperature of 20 to 80° C. for 1 to 30 minutes; thereby obtaining a high-flux, anti-fouling nanofiltration membrane;
[0043] The polyacid chloride solution comprises polyacid chloride and an organic solvent;
[0044] The polyacyl chloride is selected from at least one of 1,3,5-trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, azelayl chloride, adipic acid chloride, and 2,2',4,4'-biphenyltetracarboxylic acid chloride; the concentration of the polyacyl chloride in the polyacyl chloride solution is 0.25-7.5 mg / ml;
[0045] The organic solvent is selected from at least one of hexane, heptane, pentane, Isopar G, toluene, ethyl acetate and benzene.
[0046] The separation layer thickness of the prepared high-flux anti-scaling loose nanofiltration membrane is 8 to 230 nm, and it has a smooth structure; the MWCO of the high-flux anti-scaling loose nanofiltration membrane reaches 350 to 500 Da, and the pore radius reaches 0.45 to 0.55 nm; the carboxyl density of the high-flux anti-scaling loose nanofiltration membrane reaches 0.8 to 1.5 sites·nm -3 ;
[0047] The pure water flux of the prepared high-flux anti-fouling loose nanofiltration membrane is 40L·h -1 ·m -2 bar -1As mentioned above, the retention rates of tetracycline and norfloxacin reached over 96%; the retention rate of PEG600 reached over 96%; under the premise of ensuring high retention rate of specific substances, the water flux and anti-scaling performance were improved.
[0048] The high-flux anti-scaling loose nanofiltration membrane prepared by the invention can be applied to sewage treatment.
[0049] The following are specific embodiments
[0050] Example 1
[0051] The pH value of a mixed aqueous solution of piperazine (2.5 mg / ml) and sodium sulfate (0.1 M) was adjusted to 11.0, and a 150 KDa polysulfone substrate membrane was soaked in the solution for 120 seconds, and then dried in the air until there was no obvious water stain on the membrane surface, thereby obtaining an ultrafiltration substrate membrane fully infiltrated with the aqueous solution; a 2 mg / ml 1,3,5-benzene trimesoyl chloride hexane solution was poured on the surface of the infiltrated substrate membrane to carry out an interfacial polymerization reaction at a reaction temperature of 25°C and a relative humidity of 80%. After reacting for 60 seconds, the membrane was taken out, washed with n-hexane, and placed in an oven and heated at 60°C for 1 minute to obtain a high-flux anti-fouling loose nanofiltration membrane. SEM and AFM analysis showed that the surface of the nanofiltration membrane had a relatively smooth structure (such as Figure 1 The separation layer thickness is ∼40 nm, and the carboxyl density is 1.02 sites·nm at pH 10.5. -3 ;
[0052] The prepared nanofiltration membrane was tested with aqueous solution cross-flow at 25°C, first refluxed at 4 bar pressure for 30 min, and then tested at 2 bar pressure. The flux was 42 L·h -1 ·m -2 bar -1; Cross-flow test with 1000ppm Na2SO4 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 97.5%; Cross-flow test with 1000ppm MgSO4 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 85.1%; Cross-flow test with 1000ppm MgCl2 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 30.8%; Cross-flow test with 1000ppm CaCl2 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 25.2%; In the cross-flow test with NaCl aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 20.5%; in the cross-flow test with 100ppm tetracycline aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 97.2%; in the cross-flow test with 100ppm norfloxacin aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 96.7%; in the cross-flow test with 1000ppm PEG600 aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 97.8%.
[0053] Comparative Example 1
[0054] After the polysulfone substrate membrane was soaked in piperazine (2.5 mg / ml) aqueous solution for 120 seconds, it was dried in the air until there was no obvious water stain on the membrane surface, and the ultrafiltration substrate membrane fully infiltrated with the aqueous solution was obtained; a 2 mg / ml 1,3,5-benzene trimesoyl chloride hexane solution was poured on the surface of the infiltrated substrate membrane to carry out interfacial polymerization reaction. The reaction temperature was 25°C and the relative humidity was 80%. After the reaction was carried out for 60 seconds, the membrane was taken out and washed with n-hexane. The membrane was placed in an oven and heated at 60°C for 1 minute to obtain a conventional nanofiltration membrane. SEM showed that the membrane surface had a dense dot structure (such as Figure 2 As shown, compared with Example 1, the membrane surface is smooth and substances are not easy to adhere to, which shows a certain anti-scaling advantage from the membrane structure; the separation layer thickness of the conventional nanofiltration membrane is ~120nm, and the carboxyl density is 0.52sites·nm at pH10.5. -3 ;
[0055] The conventional nanofiltration membrane prepared above was tested with aqueous solution cross-flow at a temperature of 25°C. It was first refluxed at a pressure of 4 bar for 30 min and then tested at a pressure of 2 bar. The flux was 24.1 L·h -1 ·m -2 bar -1; Cross-flow test with 1000ppm Na2SO4 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 98.9%; Cross-flow test with 1000ppm MgSO4 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 99.3%; Cross-flow test with 1000ppm MgCl2 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 88.7%; Cross-flow test with 1000ppm CaCl2 aqueous solution, test temperature is 25℃, test under 2bar pressure, the retention rate is 81.0%; In the cross-flow test with NaCl aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 20.5%; in the cross-flow test with 100ppm tetracycline aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 98.1%; in the cross-flow test with 100ppm norfloxacin aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 96.9%; in the cross-flow test with 1000ppm PEG600 aqueous solution, the test temperature was 25°C and the test was under a pressure of 2bar, and the retention rate was 98.6%.
[0056] Anti-scaling test
[0057] The anti-scaling experiment of Example 1 and Comparative Example 1 includes the following steps: First, the nanofiltration membranes prepared in the above two embodiments are placed in the NF cross-flow unit respectively, and refluxed for 30 minutes at a pressure of 4 bar for compaction; the cross-flow velocity and the feed solution temperature are 21.4 cm / s and 25.0±0.5°C respectively; a mixed solution consisting of 30 mM calcium chloride, 20 mM sodium sulfate and 10 mM sodium chloride is prepared, the pH of the mixed solution is adjusted to 7.0±0.1, the solution is completely mixed, and the circulation is refluxed for 1 hour. The pressure is adjusted to an appropriate pressure, and the initial permeation flux of the two membranes is 85 LMH. It is carried out at a circulation temperature of 15.0 cm / s and 25.0±0.5°C for 12 hours.
[0058] After 12 hours, the flux of the nanofiltration membrane prepared in Comparative Example 1 decreased by 27.6%, and the flux of the nanofiltration membrane prepared in Example 1 decreased by 12.7%. The nanofiltration membrane prepared in Example 1 had a smaller flux decrease, indicating that it had better anti-scaling performance.
[0059] In summary, we can draw the following conclusions:
[0060] The base membranes used in Example 1 and Comparative Example 1 are both polysulfone base membranes. In Example 1, inorganic salts are used, and the anions interact with piperazine to regulate the diffusion rate of piperazine during the interfacial polymerization process, thereby regulating the interfacial polymerization reaction, affecting the physical and chemical properties of the nanofiltration membrane separation layer, and preparing a high-flux anti-scaling loose nanofiltration membrane; the nanofiltration membrane prepared in Example 1 has a high pure water flux, a low retention rate for scaling ions, and a relatively high retention rate for antibiotics and PEG600, so it is very suitable for treating antibiotic-contaminated water sources under high recovery conditions. Comparative Example 1 does not use inorganic salts, the nanofiltration membrane separation layer is thicker and has a lower electronegativity, and the flux and anti-scaling performance are low.
Claims
1. A method for preparing a high-throughput anti-fouling loose nanofiltration membrane, characterized in that: The steps include: S1. Add an inorganic salt solution to the aqueous polyamine solution and adjust the pH value to 10 to 11.5 to obtain an interfacial polymerization aqueous solution; S2. The ultrafiltration base membrane for the experiment is fully infiltrated with the interfacial polymerization aqueous solution, and then dried in the air until there is no obvious water stain on the membrane surface, thereby obtaining an ultrafiltration base membrane fully infiltrated with the aqueous solution; S3. Pour the oil phase solution onto the surface of the aqueous ultrafiltration base membrane, so that the polyacyl chloride solution is fully in contact with the aqueous polyamine monomer, and the polymerization reaction occurs sufficiently, thereby forming a layer of polyamide ultrathin film on the aqueous ultrafiltration base membrane; The polyacid chloride solution comprises polyacid chloride and an organic solvent; S4. The prepared polyamide membrane is annealed to obtain a high-flux anti-fouling loose nanofiltration membrane.
2. The preparation method according to claim 1, characterized in that: In step S1, the inorganic salt is selected from one or more of a fluoride salt system, a bromide salt system, a nitrate system, a silicate system, a tungstate system, a molybdate system, a permanganate system, a sulfate system, a sulfite system and a pyrophosphate system; and the concentration of the inorganic salt in the interfacial polymerization aqueous phase solution is 0.01 to 0.5 M.
3. The preparation method according to claim 1, characterized in that: In step S1, the polyamine solution is prepared by adding a polyamine monomer into water, wherein the polyamine monomer is selected from at least one of piperazine, m-phenylenediamine, p-phenylenediamine, melamine, thiourea, polyethyleneimine, diethyltriamine and N-aminoethylpiperazine.
4. The preparation method according to claim 1, characterized in that: In step S2, the ultrafiltration base membrane material is selected from any one of polysulfone, polyethersulfone, polyvinylidene fluoride, polyacrylonitrile, polytetrafluoroethylene nylon, cellulose or cellulose derivatives; the pore size of the ultrafiltration base membrane is 0.01 to 2 μm.
5. The preparation method according to claim 1, characterized in that: In step S3, the organic solvent is selected from at least one of hexane, heptane, pentane, Isopar G, toluene, ethyl acetate and benzene.
6. The preparation method according to claim 1, characterized in that: In step S3, the polyacyl chloride is selected from at least one of 1,3,5-trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, azelayl chloride, adipic acid chloride, and 2,2',4,4'-biphenyltetracarboxylic acid chloride; and the concentration of the polyacyl chloride in the polyacyl chloride solution is 0.25-7.5 mg / ml.
7. The preparation method according to claim 1, characterized in that: In step S3, the polyamine monomer and the polyacyl chloride are subjected to an interfacial polymerization reaction at an interface temperature of 20 to 35° C. and a relative humidity of 50 to 100% for 30 to 90 seconds.
8. The preparation method according to claim 1, characterized in that: In step S4, the annealing treatment is performed at a temperature of 20 to 80° C. for 1 to 30 minutes.
9. A high-flux anti-scaling loose nanofiltration membrane prepared by any one of the preparation methods of claims 1-8, characterized in that: The separation layer thickness of the high-flux anti-scaling loose nanofiltration membrane is 8 to 230 nm, and has a smooth structure; the MWCO of the high-flux anti-scaling loose nanofiltration membrane reaches 350 to 500 Da, and the pore radius reaches 0.45 to 0.55 nm; the carboxyl density of the high-flux anti-scaling loose nanofiltration membrane reaches 0.8 to 1.5 sites·nm -3 ; The pure water flux of the high-flux anti-scaling loose nanofiltration membrane is 40 L·h -1 ·m -2 bar -1 As shown above, the retention rates of tetracycline and norfloxacin reached over 96%; the retention rate of PEG600 reached over 96%.
10. Use of the high-flux anti-scaling loose nanofiltration membrane in water treatment according to claim 9, characterized in that: The high-flux anti-scaling loose nanofiltration membrane is applied to sewage treatment.
Citation Information
Cited By
High-water-flux thin-layer composite nanofiltration membrane and preparation method thereof
CN120268255A
High-flux nanofiltration membrane with narrow pore size distribution, preparation method of high-flux nanofiltration membrane and new pollutant treatment method
CN121130675A