MAX-phase ceramic-metal-high-temperature alloy-based self-lubricating composite shaft sleeve and preparation method thereof
By filling the MAX-phase ceramics and metal components in the high-temperature alloy sleeve, a self-lubricating structure is formed, which solves the problem of insufficient mechanical and frictional properties of traditional lubricating materials in high-temperature environments, and achieves the coordination and unity of high-temperature mechanical properties and self-lubricating effects. , suitable for bearing systems for heavy-duty equipment.
Patent Information
- Application Number
- CN202411157537.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Traditional liquid and solid lubricating materials cannot meet the high temperature, high strength and low friction requirements of heavy equipment under high-temperature and heavy-duty friction environments, and existing metal alloys and ceramic composites are difficult to achieve the coordination and unity of high-temperature mechanics and friction performance.
Using MAX phase ceramic-metal-high temperature alloy-based self-lubricating composite shaft sleeve, the self-lubricating structure is formed by setting a housing cavity in the main structure of the high temperature alloy shaft sleeve, and filling the MAX phase metal cermet components and metal components to form a self-lubricating structure, and sintering treatment is performed. It forms a metallurgical reaction combination, forming a strong interface combination to ensure the mechanical properties and self-lubricating effect of the shaft sleeve at high temperatures.
The composite shaft sleeve with good high-temperature mechanical properties, high-temperature stability and high-temperature lubrication and wear resistance can provide effective wide-temperature support, lubrication and protection in extreme high-temperature environments and extend service life.
Smart Images

Figure CN119035555A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of shaft sleeves, and in particular to a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite shaft sleeve and a preparation method thereof. Background Art
[0002] In recent years, the rapid development of heavy equipment such as generators, engines, and gas turbines has brought a series of new challenges to the service performance of sliding bearing assemblies. This is particularly true for key components such as internal sleeves, bushings, and piston rings, which face long-term, oil-free service at temperatures exceeding 600°C and high-friction environments with complex, high-stress loads. To ensure the proper support, stability, and lifespan of shaft components, these sleeves must possess both high-temperature strength and high-temperature anti-friction properties. However, conventional liquid and solid lubricants often lack high-temperature mechanical properties, failing to meet the demands of high-temperature, heavy-load, and frictional environments. Therefore, the research and development of a new generation of high-temperature solid-lubricant sleeves capable of operating in complex environments such as high temperature, high pressure, and high loads is urgent. Currently reported solid-lubricant sleeves based on metal alloys, ceramics, and composite materials have struggled to achieve a balanced balance of high-temperature mechanical and tribological properties. Therefore, a new metal-based self-lubricating sleeve with both high-temperature strength and low friction is urgently needed to meet these high-temperature, high-load service requirements. Summary of the Invention
[0003] The object of the present invention is to provide a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite shaft sleeve having both good high temperature mechanical properties and high temperature self-lubricating properties and a preparation method thereof.
[0004] In a first aspect, the present invention provides a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve, the composite sleeve comprising a sleeve main structure and a self-lubricating structure, the sleeve main structure being provided with a receiving cavity to be filled, the self-lubricating material being filled and compounded in the receiving cavity of the sleeve main structure to form the self-lubricating structure;
[0005] Wherein, the main structure of the sleeve is made of a high-temperature alloy material, and the high-temperature alloy material includes at least one of Ni-based, Co-based, Fe-based, Ti-based, Mo-based, Nb-based or intermetallic compound-based high-temperature alloys;
[0006] The self-lubricating material includes a MAX phase cermet component and a metal component;
[0007] The molecular formula of the MAX phase metal ceramic component is M n+1 AX n, n=1, 2 or 3, M includes at least one of Ti, V, Cr, Zr, Nb, Mo, Hf, Sc or Ta, A includes at least one of Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl or Pb, and X is C and / or N;
[0008] The metal component includes at least one of Cu, Ag, Pb, Ti, Al or V.
[0009] Optionally, the accommodating cavity includes at least one of a hole, a groove or an interpenetrating network pore structure provided on the main structure of the sleeve, and the total volume of the accommodating cavity accounts for 10 to 70% of the total volume of the main structure of the sleeve.
[0010] Optionally, the total volume of the accommodating cavity accounts for 20% to 50% of the total volume of the sleeve main body structure.
[0011] Optionally, the mass ratio of the MAX phase metal ceramic component to the metal component is 0.5:99.5 to 99.5:0.5.
[0012] Optionally, the high-temperature alloy material includes a Ni-based high-temperature alloy.
[0013] Optionally, the MAX phase metal ceramic component includes Ti3AlC2 and / or doped (Ti,M')3AlC2, wherein M' includes at least one of Cr, V, Zr or Nb; the metal component includes Cu and / or Cu-M" alloy, wherein M" includes at least one of Ni, Sn, Cr, Nb, Ag, Pb, Ti or Al.
[0014] Optionally, a transition layer is formed between the sleeve main structure and the self-lubricating structure, and the average thickness of the transition layer is 3 to 30 μm.
[0015] Optionally, the phase structure of the transition layer includes a Cu / Ni phase and a Ni / Ni3Al phase.
[0016] In a second aspect, the present invention provides a method for preparing a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve, comprising the following steps:
[0017] S1 provides a sleeve main structure and a self-lubricating material, the sleeve main structure is provided with a receiving cavity to be filled, the self-lubricating material is filled in the receiving cavity of the sleeve main structure;
[0018] S2. Sintering and molding to prepare the self-lubricating composite sleeve, wherein the self-lubricating material is compounded in the accommodating cavity of the sleeve main structure to form a self-lubricating structure.
[0019] Optionally, in step S2, the sintering pressure is 30-1000 MPa, the sintering temperature is 700-1300° C., and the holding time is 5-200 min.
[0020] Optionally, in step S2, the sintering pressure is 30-100 MPa, the sintering temperature is 850-1000° C., and the holding time is 5-30 min.
[0021] In summary, the present invention has at least one of the following beneficial effects:
[0022] 1. The present invention provides a composite shaft sleeve with good high-temperature mechanical properties, high high-temperature stability, and high-temperature lubrication and wear resistance. The high-temperature, high-strength, self-lubricating composite shaft sleeve has broad application prospects in extreme high temperature, complex load, impact, and high-temperature friction environments.
[0023] 2. The present invention realizes the metallurgical reaction bonding between the main structure of the high-temperature alloy sleeve and the MAX phase-based self-lubricating structure, and the two can form a strong interface bond. At the same time, the metallurgical bonding between the two structures ensures the synergistic performance of their respective properties and the overall strength of the composite sleeve. The prepared composite sleeve uses a high-strength high-temperature alloy as the main structure of the sleeve, ensuring that the sleeve has good mechanical properties in environments from room temperature to high temperature. The MAX phase-based self-lubricating material is filled on the friction surface of the sleeve to form a self-lubricating structure. Its own multi-layered microstructure and high-temperature stability ensure that the sleeve has good high-temperature self-lubricating effect and wear resistance on the friction surface. In summary, this type of composite sleeve has the comprehensive performance of both high-temperature alloys and high-temperature solid lubricating materials, and can effectively support, lubricate, stabilize and protect the bearing system over a wide temperature range. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0025] Figure 1 Schematic diagram of the structure of different self-lubricating composite sleeves according to the embodiment of the present invention;
[0026] Figure 2 This is a photo of the self-lubricating composite sleeve with an outer diameter of 20 mm sintered at 900°C in Example 1;
[0027] Figure 3 This is the interface microstructure of the self-lubricating composite sleeve with an outer diameter of 20 mm sintered at 900°C in Example 1;
[0028] Figure 4This is the friction coefficient curve between the inner surface of the self-lubricating composite sleeve with an outer diameter of 20 mm sintered at 900°C and the high-temperature alloy in Example 1;
[0029] Figure 5 This is the friction coefficient curve between the inner surface of the self-lubricating composite sleeve with an outer diameter of 30 mm sintered at 900°C and the high-temperature alloy in Example 2;
[0030] Figure 6 This is the interface microstructure of the self-lubricating composite sleeve with an outer diameter of 30 mm sintered at 1000°C in Example 3. DETAILED DESCRIPTION
[0031] The present invention provides a MAX phase ceramic-metal-high temperature alloy-based self-lubricating composite bushing and a method for preparing the same. To clarify the objectives, technical solutions, and effects of the present invention, the present invention is described in further detail below. It should be understood that the specific embodiments described herein are intended only to illustrate the present invention and are not intended to limit the present invention.
[0032] Superalloys are a class of metallic materials based on iron, nickel, cobalt, titanium, molybdenum, niobium, or intermetallic compounds that can operate for extended periods at temperatures exceeding 600°C and under certain stresses. They exhibit excellent high-temperature strength, high-temperature oxidation and corrosion resistance, as well as excellent fatigue performance and fracture toughness. They are primarily used in the aerospace sector. For example, as flight speeds continue to increase, engines will need to have a higher weight-to-weight ratio, increasing loads and rising ambient temperatures. This is particularly true for critical components such as sleeves, bushings, and piston rings. Lubricants and greases are easily diluted in high-temperature environments, and they face long-term service in temperatures exceeding 600°C without oil lubrication and under complex, high-stress, high-friction environments. Research reports indicate that developing wear-resistant materials with self-lubricating properties under high-temperature conditions has significant application value in improving the high-temperature wear resistance of moving parts. After long-term research, the inventors have creatively proposed a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve and its preparation method. The sleeve consists of two parts: a high temperature alloy based sleeve main structure and a self-lubricating filling structure. The sleeve main structure is a high-strength and high-temperature structural material with a straight groove, inclined groove or inner hole with a cross-section of semicircular, U-shaped, V-shaped, square, dovetail, etc. to be filled. The self-lubricating filling structure is a MAX phase ceramic (M n+1 AX nA high-temperature self-lubricating material is composed of a metal material (where M is a pre-transition metal, A is a Group A element, X is carbon and / or nitrogen, and n=1, 2, 3) and a metal material; the two are combined through a sintering process to ultimately form a composite sleeve with high-temperature, high-strength, self-lubricating properties. This ensures that the composite sleeve has high mechanical properties as a whole under high-temperature, oil-free lubrication conditions, while the friction surface still has self-lubricating, low-friction, and low-wear properties, resulting in a long service life. This type of sleeve can support, fix, protect, and lubricate the shaft in complex environments such as high temperature, oxidation resistance, and load impact, ensuring the normal operation of various operating components. The present invention is based on this.
[0033] In some embodiments of the present invention, a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve is provided, wherein the composite sleeve comprises a sleeve main body structure and a self-lubricating structure, wherein the sleeve main body structure is provided with a receiving cavity to be filled, and a self-lubricating material is filled and compounded in the receiving cavity of the sleeve main body structure to form the self-lubricating structure;
[0034] Wherein, the main structure of the sleeve is made of a high-temperature alloy material, and the high-temperature alloy material includes at least one of Ni-based, Co-based, Fe-based, Ti-based, Mo-based, Nb-based or intermetallic compound-based high-temperature alloys;
[0035] The self-lubricating material includes a MAX phase cermet component and a metal component;
[0036] The molecular formula of the MAX phase metal ceramic component is M n+1 AX n , n=1, 2 or 3, M includes at least one of Ti, V, Cr, Zr, Nb, Mo, Hf, Sc or Ta, A includes at least one of Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl or Pb, and X is C and / or N;
[0037] The metal component includes at least one of Cu, Ag, Pb, Ti, Al or V. The metal may be a single metal or an alloy.
[0038] In some embodiments of the present invention, the intermetallic compound-based high-temperature alloy includes at least one of a Ni3Al-based intermetallic compound high-temperature alloy, a NiAl-based intermetallic compound high-temperature alloy, a Ti3Al-based intermetallic compound high-temperature alloy, a TiAl-based intermetallic compound high-temperature alloy, and a Fe3Al-based intermetallic compound high-temperature alloy.
[0039] In some embodiments of the present invention, the high-temperature alloy material includes a Ni-based high-temperature alloy; preferably, the MAX phase metal ceramic component M includes at least one of Ti, V, Cr, Zr, and Nb; A includes at least one of Al, Si, P, S, Ga, or Pb; more preferably, the MAX phase metal ceramic component includes Ti3AlC2 and / or doped (Ti,M')3AlC2, wherein M' includes at least one of Cr, V, Zr, or Nb; the metal component includes Cu and / or Cu-M" alloy, wherein M" includes at least one of Ni, Sn, Cr, Nb, Ag, Pb, Ti, or Al; more preferably, the MAX phase metal ceramic component includes Ti3AlC2, and the metal component includes Cu.
[0040] In some embodiments of the present invention, the accommodating cavity includes at least one of a hole, a groove or an interpenetrating network pore structure arranged on the sleeve main body structure, and the total volume of the accommodating cavity accounts for 10 to 70% of the total volume of the sleeve main body structure; preferably, the total volume of the accommodating cavity accounts for 20 to 50% of the total volume of the sleeve main body; more preferably, the total volume of the accommodating cavity accounts for 25 to 40% of the total volume of the sleeve main body; more preferably, the total volume of the accommodating cavity accounts for 26 to 33% of the total volume of the sleeve main body.
[0041] In some embodiments of the present invention, the mass ratio of the MAX phase metal ceramic component to the metal component is 0.5:99.5 to 99.5:0.5; preferably, the mass ratio of the MAX phase metal ceramic component to the metal component is 20:80 to 80:20; more preferably, the mass ratio of the MAX phase metal ceramic component to the metal component is 30:70 to 70:30.
[0042] In some embodiments of the present invention, a transition layer is formed between the sleeve main structure and the self-lubricating structure, and the average thickness of the transition layer is 3 to 30 μm; preferably, the average thickness of the transition layer is 5 to 20 μm; more preferably, the average thickness of the transition layer is 8 to 12 μm.
[0043] In some embodiments of the present invention, the phase structure of the transition layer includes a Cu / Ni phase and a Ni / Ni3Al phase.
[0044] In some embodiments of the present invention, a method for preparing a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite bushing is provided, comprising the following steps:
[0045] S1 provides a sleeve main structure and a self-lubricating material, the sleeve main structure is provided with a receiving cavity to be filled, the self-lubricating material is filled in the receiving cavity of the sleeve main structure;
[0046] S2. Sintering and molding to prepare the self-lubricating composite sleeve, wherein the self-lubricating material is compounded in the accommodating cavity of the sleeve main structure to form a self-lubricating structure.
[0047] In some embodiments of the present invention, in step S2, the sintering pressure is 30-1000 MPa, the sintering temperature is 700-1300°C, and the holding time is 5-200 min; preferably, the sintering pressure is 30-100 MPa, the sintering temperature is 850-1000°C, and the holding time is 5-100 min; more preferably, the sintering pressure is 40-80 MPa, the sintering temperature is 870-970°C, and the holding time is 5-20 min.
[0048] In some embodiments of the present invention, please refer to Figure 1 , Figure 1 The figure shows a schematic diagram of the structure of a possible composite sleeve. The composite sleeve includes a sleeve main structure and a self-lubricating structure. The sleeve main structure is a circular ring structure, and the inner surface is provided with straight grooves, inclined grooves or porous accommodating cavities to be filled with cross-sections of semicircular, U-shaped, V-shaped, square, etc.; the self-lubricating material is filled in the accommodating cavity of the sleeve main structure. The self-lubricating material includes a MAX phase metal ceramic component and a metal component. After the filling is completed, sintering is performed to prepare the composite sleeve. The self-lubricating material is compounded in the accommodating cavity of the sleeve main structure to form a self-lubricating structure.
[0049] In some embodiments of the present invention, the MAX phase metal ceramic component can be a pure metal ceramic, or it can be doped with a small amount of a second type of compound, which includes nitrides (Si3N4, AlN, etc.), borides (TiB2, ZrB2, etc.), oxides (Al2O3, MoO3), sulfides (MoS2, WS2, etc.) or intermetallic compounds (Ti3Al, Ni3Al, etc.). The addition of a hard, difficult-to-oxidize second type of compound with a high melting point and high shear strength will play a role in dispersion strengthening, improving the strength of the composite sleeve at high temperatures. However, during the friction process, it may be released under the action of the grinding pair, forming abrasive particles, thereby increasing the volume wear rate of the composite sleeve. The addition of a low-melting-point oxide or a second type of compound that oxidizes to form a low-melting-point oxide during the friction process will improve the self-lubricating properties of the composite sleeve. For example, TiB2 will form B3O2 during high-temperature friction, reducing the friction coefficient and volume wear rate.
[0050] The present invention is further described below with reference to specific examples. Unless otherwise specified, the raw materials in the specific examples of the present invention are commercially available or obtained by conventional preparation methods in the art.
[0051] Example 1
[0052] This embodiment provides a MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve and a preparation method thereof, comprising the following steps:
[0053] S1. Provide a shaft sleeve main structure and self-lubricating material. The shaft sleeve main structure is made of high-temperature alloy material. The high-temperature material of Example 1 adopts Incol738 nickel-based high-temperature alloy. The outer diameter of the shaft sleeve main body is 20 mm, the inner diameter is 16 mm, and the height is 3 mm. The inner ring of the shaft sleeve main structure is provided with evenly distributed accommodating cavities. The accommodating cavities are machined to form inner grooves with a semicircular cross-section, a spacing of 0.1 mm, and a semicircular diameter of 1.5 mm. The total volume of the accommodating cavities accounts for 30% of the total volume of the shaft sleeve main structure.
[0054] The self-lubricating material used in Example 1 is a uniform mixture of Ti3AlC2 powder and Cu powder, wherein the mass ratio of Ti3AlC2 powder to Cu powder is 40:60, the particle sizes of Ti3AlC2 powder and Cu powder are 5 μm and 10 μm respectively, and the purity of both is above 99.9%.
[0055] The self-lubricating material is filled into the accommodating cavity of the main structure of the sleeve, specifically including the following steps: at room temperature, a mold with an inner diameter of 20.3 mm and a height of 10 mm is selected, the mold includes upper and lower punches and an outer mold, the lower punch is placed in the outer mold, and the mixed powder of the self-lubricating material is filled in, the main structure of the sleeve is placed in the mold, and then the mixed powder of the self-lubricating material is filled in, and then the upper punch is placed in the mold, followed by cold pre-pressing, the cold pressing strength is 100 MPa, and the filling amount of the self-lubricating material is 30% of the total volume of the main structure of the sleeve.
[0056] S2. Sintering molding: Place the pre-pressed mold into a spark plasma sintering furnace for sintering at a temperature of 950°C. Maintain vacuum in the furnace with a vacuum degree of 10 -3 Pa, the holding time is 10min, the sintering pressure is 50MPa, and after holding, it is cooled to room temperature and taken out to prepare the composite shaft sleeve. Figure 2 As shown, after demoulding, the density of the sintered nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve was measured to be greater than 99%.
[0057] Scanning electron microscopy (SEM) was used to characterize the microstructure of the composite sleeve prepared in Example 1. The microstructure of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 1 is as follows: Figure 3 As shown, from Figure 3As can be seen in the figure, the region marked 3 is the Ni-based superalloy, the region marked 2 is the transition layer, and the region marked 1 is the MAX-based self-lubricating material. The average thickness of the transition layer is 10μm. The measured phase structure of the transition layer consists of Cu / Ni and Ni / Ni3Al phases. The main structure of the Ni-based superalloy sleeve and the MAX-based self-lubricating structure are tightly integrated without any gaps. Nanoindentation measurements show that the hardness corresponding to points 1, 2, and 3 in the figure are 7.6GPa, 7.3GPa, and 5.7GPa, respectively.
[0058] The radial crushing strength of the composite sleeve prepared in Example 1 was tested using a pressure testing machine. The crushing strengths of the nickel-based superalloy / Ti3AlC2+Cu composite sleeve in Example 1 were 1050 MPa at room temperature and 630 MPa at 800°C, respectively. This demonstrates that the nickel-based superalloy / Ti3AlC2+Cu composite sleeve prepared in Example 1 has excellent mechanical properties at both room temperature and high temperature.
[0059] The friction coefficient of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 1 was tested in air at room temperature and 800°C using an American Brook friction tester. The friction pair was a high-temperature alloy friction pair, a high-temperature alloy GH4169 ball was used, the friction load was 10N, and the test surface was the inner surface of the composite sleeve. The friction coefficient curve is shown in FIG. Figure 4 The average friction coefficient of the composite bushing prepared in Example 1 was measured to be 0.390 at room temperature, and the wear rate was 8.03×10 -5 mm 3 / (N·m); the average friction coefficient at high temperature of 800℃ is 0.185, and the wear rate is 6.56×10 -6 mm 3 The experimental results show that the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 1 has excellent self-lubricating properties during the friction process from room temperature to 800°C.
[0060] Example 2
[0061] Example 2 differs from Example 1 in that, in step S1, the main structure of the high-temperature alloy sleeve has an outer diameter of 30 mm, an inner diameter of 23 mm, and a height of 3 mm. The inner ring of the sleeve body is provided with evenly distributed accommodating cavities, each with a semicircular cross-section and a spacing of 0.1 mm. The semicircular diameter is 2 mm, and the total volume of the accommodating cavities accounts for 30% of the total volume of the sleeve body. The mold used has an inner diameter of 30.3 mm. The remaining preparation steps are the same as in Example 1. A nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve is produced. The density of the sintered nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve is measured to be greater than 99%.
[0062] The microstructure of the nickel-based superalloy / Ti3AlC2+Cu composite sleeve prepared in Example 2 was characterized using the same testing methods as in Example 1. Measurements showed that the nickel-based superalloy / Ti3AlC2+Cu composite sleeve prepared in Example 2 consisted of a Ni-based superalloy, a transition layer, and a MAX-based self-lubricating material. The transition layer had an average thickness of 10 μm and consisted of a Cu / Ni phase and a Ni / Ni3Al phase. The main structure of the Ni-based superalloy sleeve and the MAX-based self-lubricating structure were tightly integrated without any gaps.
[0063] The same method as in Example 1 was used to test the crushing strength of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 2. The crushing strength of the composite sleeve of Example 2 was measured to be 1211 MPa and 864 MPa at room temperature and 800°C, respectively. It can be seen that the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 2 has excellent mechanical properties at room temperature and high temperature, and is significantly better than that of Example 1. It is speculated that the reason for the improved crushing strength of Example 2 compared with Example 1 is due to the improved strength of the main structure of the high-temperature alloy sleeve.
[0064] The friction coefficient of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 2 was tested in the same manner as in Example 1 at room temperature, 600°C and 800°C in air. The friction coefficient curves are shown in FIG. Figure 5 The average friction coefficient of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 2 was 0.396 at room temperature, and the wear rate was 9.20×10 -5 mm 3 / (N·m); the average friction coefficient at 600℃ is 0.303, and the wear rate is 5.19×10 -5 mm 3 / (N·m); the average friction coefficient at 800℃ is 0.291, and the wear rate is 5.69×10 -6 mm 3 The experimental results show that the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve of Example 2 has excellent room temperature and high temperature self-lubricating properties, and has no significant change compared to the self-lubricating properties of Example 1.
[0065] Example 3
[0066] Example 3 differs from Example 2 in that the sintering temperature in step S2 of Example 3 is 1000°C. The remaining preparation steps are the same as in Example 2, resulting in a nickel-based superalloy / Ti3AlC2+Cu composite shaft sleeve. The density of the sintered nickel-based superalloy / Ti3AlC2+Cu composite shaft sleeve was measured to be greater than 99%.
[0067] The microstructure of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Test Example 3 is as follows: Figure 6 As shown, the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 3 includes a Ni-based high-temperature alloy, a transition layer, metal Cu, and a layered structure Ti3AlC2 dispersed in the metal Cu. The average thickness of the transition layer is 15 μm, and the composition of the transition layer includes Cu / Ni phase and Ni / Ni3Al phase. The main structure of the Ni-based high-temperature alloy sleeve and the MAX-based self-lubricating structure are tightly combined without gaps.
[0068] The crushing strength of the composite sleeve of Example 3 was tested by the same method as that of Example 2. The crushing strength of the composite sleeve of Example 3 was measured to be 1179 MPa and 659 MPa at room temperature and 800°C, respectively. It can be seen that the composite sleeve prepared in Example 3 has good mechanical properties at room temperature and high temperature, but the mechanical properties are significantly reduced compared with those of Example 2. It is speculated that the reason for the decrease in strength is that the volume fraction of the γ' phase of the nickel-based high-temperature alloy is reduced during high-temperature sintering.
[0069] The friction performance of the composite bushing prepared in Example 3 was tested using the same method as in Example 2. The average friction coefficient of the composite bushing prepared in Example 3 was 0.48 at room temperature, and the wear rate was 1.2×10 -4 mm 3 / (N·m); the average friction coefficient at high temperature of 800℃ is 0.28, and the wear rate is 8*10 -6 mm 3 / (N·m). The experimental results show that the composite bushing prepared in Example 3 has good self-lubricating properties at room temperature and high temperature, but the self-lubricating performance is significantly reduced compared with that in Example 2. It is speculated that the main reason is that the reaction between Ti3AlC2 and the nickel-based high-temperature alloy increases at high temperature, the width of the generated transition layer increases, and more hard Ni3Al is formed, which reduces the room temperature lubrication performance.
[0070] Example 4
[0071] The difference between Example 4 and Example 2 is that the total volume of the accommodating cavity in Example 4 accounts for 35% of the total volume of the main structure of the sleeve, the filling amount of the self-lubricating material is 35% of the total volume of the main structure of the sleeve, and the remaining preparation steps are the same as Example 2 to prepare a nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve.
[0072] The microstructure of the nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 4 was tested and characterized using the same method as in Example 2. The nickel-based high-temperature alloy / Ti3AlC2+Cu composite sleeve prepared in Example 4 was found to comprise a nickel-based high-temperature alloy, a transition layer, metallic Cu, and a layered Ti3AlC2 structure dispersed in the metallic Cu. The transition layer had an average thickness of 15 μm and consisted of a Cu / Ni phase and a Ni / Ni3Al phase. The main structure of the nickel-based high-temperature alloy sleeve and the MAX-based self-lubricating structure were tightly integrated without gaps.
[0073] The same method as in Example 2 was used to test the crushing strength of the composite sleeve of Example 4, and the crushing strength was significantly lower than that of Example 2. The same method as in Example 4 was used to test the lubrication performance of Example 4, and the self-lubricating performance of Example 4 was significantly lower than that of Example 2. It is speculated that the main reason is that the increase in the filling amount of the self-lubricating material leads to a decrease in mechanical properties, and the average width of the transition layer increases, resulting in the formation of more hard Ni3Al, which reduces the self-lubricating performance.
[0074] Example 5
[0075] Example 5 differs from Example 2 in that, in step S1 of Example 5, a porous or honeycomb-structured sleeve is manufactured using Incol 738 high-temperature alloy powder through additive manufacturing. This structure features evenly distributed circular holes and honeycomb grooves within the inner ring. At room temperature, the high-temperature alloy sleeve body is placed in a cemented carbide mold and filled with a mixed powder of copper and Ti3AlC2 phase cermet. The mold is then sintered in a spark plasma sintering furnace at 900°C, maintained in a vacuum, and cooled to room temperature. This produces a composite sleeve.
[0076] Through the above preparation process, the embodiments of the present invention can obtain a high-temperature alloy-based high-temperature solid lubricating composite shaft sleeve that is dense, has good mechanical properties, is resistant to high temperatures, and has good self-lubricating effect, especially embodiments 1 and 2 have excellent self-lubricating performance.
[0077] It should be understood that the application of the present invention is not limited to the above examples. For those skilled in the art, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve, characterized in that: The composite sleeve comprises a sleeve main structure and a self-lubricating structure, wherein the sleeve main structure is provided with a receiving cavity to be filled, and the self-lubricating material is filled and compounded in the receiving cavity of the sleeve main structure to form the self-lubricating structure; Wherein, the main structure of the sleeve is made of a high-temperature alloy material, and the high-temperature alloy material includes at least one of a Ni-based, Co-based, Fe-based, Ti-based, Mo-based, Nb-based or intermetallic compound-based high-temperature alloy; The self-lubricating material comprises a MAX phase cermet component and a metal component; The molecular formula of the MAX phase metal ceramic component is M n+1 AX n , n=1, 2 or 3, M includes at least one of Ti, V, Cr, Zr, Nb, Mo, Hf, Sc or Ta, A includes at least one of Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl or Pb, and X is C and / or N; the metal component includes at least one of metal Cu, Ag, Pb, Ti, Al or V.
2. The MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve according to claim 1, characterized in that: The accommodating cavity includes at least one of a hole, a groove or an interpenetrating network pore structure arranged on the main structure of the sleeve, and the total volume of the accommodating cavity accounts for 10-70% of the total volume of the main structure of the sleeve.
3. The MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve according to claim 2, characterized in that: The total volume of the accommodating cavity accounts for 20-50% of the total volume of the sleeve main structure.
4. The MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve according to claim 1, characterized in that: The mass ratio of the MAX phase metal ceramic component to the metal component is 0.5:99.5 to 99.5:0.
5.
5. The MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve according to any one of claims 1 to 4, characterized in that: The high temperature alloy material includes a Ni-based high temperature alloy.
6. The MAX phase ceramic-metal-high temperature alloy based self-lubricating composite bushing according to any one of claims 1 to 4, characterized in that: The MAX phase metal ceramic component includes Ti3AlC2 and / or doped (Ti,M')3AlC2, wherein M' includes at least one of Cr, V, Zr or Nb; the metal component includes Cu and / or Cu-M" alloy, wherein M" includes at least one of Ni, Sn, Cr, Nb, Ag, Pb, Ti or Al.
7. The MAX phase ceramic-metal-high temperature alloy based self-lubricating composite bushing according to claim 6, characterized in that: A transition layer is formed between the shaft sleeve main body structure and the self-lubricating structure, and the average thickness of the transition layer is 3 to 30 μm.
8. A method for preparing the MAX phase ceramic-metal-high temperature alloy based self-lubricating composite bushing according to any one of claims 1 to 7, characterized in that: The steps include: S1. Providing a sleeve main structure and a self-lubricating material, wherein the sleeve main structure is provided with a receiving cavity to be filled, and the self-lubricating material is filled in the receiving cavity of the sleeve main structure; S2. Sintering and molding to prepare the self-lubricating composite sleeve, wherein the self-lubricating material is compounded in the accommodating cavity of the sleeve main structure to form a self-lubricating structure.
9. The method for preparing the MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve according to claim 8, characterized in that: In step S2, the sintering pressure is 30-1000 MPa, the sintering temperature is 700-1300° C., and the holding time is 5-200 min.
10. The method for preparing the MAX phase ceramic-metal-high temperature alloy based self-lubricating composite sleeve according to claim 9, characterized in that: In step S2, the sintering pressure is 30-100 MPa, the sintering temperature is 850-1000° C., and the holding time is 5-30 min.
Citation Information
Patent Citations
Ni-base alloy / ceramic composite material and preparing method thereof
CN105648276A
High-temperature bionic self-lubricating hot work die material and preparation method thereof
CN107520446A
MAX-phase reinforced copper-based composite material and preparation method thereof
CN108913932A
Ceramic-metal bionic nanocomposite material and preparation method thereof
CN113277851A
Metal-based self-lubricating composite material as well as preparation method and application thereof
CN118374712A
Cited By
High-temperature high-strength self-lubricating composite material and preparation method thereof
CN119016730A
A high-temperature, high-strength, self-lubricating composite material and preparation method thereof
CN119016730B
High-temperature and high-strength self-lubricating composite material and preparation method therefor
WO2026041172A1