Preparation method of low-stress high-precision optical glass

By reasonably preparing raw materials such as phosphorus pentoxide, barium oxide, etc. in optical glass and performing multiple steps to solve the problem of insufficient chemical stability and hardness when increasing the refractive index, the high refractive index and excellent permeability are achieved Optical performance and high mechanical strength meet the needs of high-precision imaging applications.

CN119038876APending Publication Date: 2024-11-29SETH (TAICANG) MATERIAL TECH CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411229598.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional optical glasses may lead to reduced chemical stability or insufficient hardness when increasing the refractive index, resulting in insufficient light transmission performance and inability to meet the high requirements of high-precision imaging applications.

Method used

Using low-stress and high-precision optical glass preparation method, melting, forming, annealing, polishing and coating by mixing raw materials such as phosphorus pentoxide, barium oxide, aluminum oxide, zinc oxide, zirconium oxide, boron trioxide and nano-silicon powder. Treatment, controls the chemical composition and structure of the glass to ensure the chemical stability and optical properties of the glass.

Benefits of technology

The high refractive index, excellent light transmission performance and high mechanical strength of the glass are achieved, the internal stress is reduced, the stability and imaging quality of the glass are improved, the service life is extended, and the high precision and flatness are ensured through coating treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038876A_ABST
    Figure CN119038876A_ABST
Patent Text Reader

Abstract

The invention relates to the field of optical glass, and discloses a preparation method of low-stress high-precision optical glass, which comprises the following steps: S1, preparing raw materials; s2, mixing the raw materials: putting the prepared glass raw materials into a mixing device, and mixing the glass raw materials with 2, 2 '-bis (2, 4-Dimethylphenyl) pentaoxide; adding the mixture into a mixing device, adding zirconium oxide into the mixing device, and finally adding titanium dioxide or nano silicon powder into the mixing device for mixing; s3, smelting is conducted; s4, forming and annealing; s5, polishing is conducted; s6, surface cleaning; and S7, coating treatment is carried out. The chemical stability can be improved and the refractive index can be adjusted through phosphorus pentoxide; barium oxide increases the refractive index; after the glass raw materials are mixed, the cost performance of the optical glass is high, batch production is easy to realize, the optical glass has excellent light transmission performance, the refractive index of the optical glass is further improved by adding the nano titanium dioxide or the nano silicon powder, and the optical glass is good in chemical stability and suitable for high-precision imaging mirror surfaces. An optical system is simplified and imaging quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of optical glass, in particular to a method for preparing low-stress high-precision optical glass. Background Art

[0002] High-precision optical glass is a type of glass material with excellent optical properties. It is widely used in various optical systems, such as camera lenses, microscopes, telescopes, and laser systems. Its main features include high transparency, low optical distortion, and high wear resistance. Low-stress high-precision optical glass is a specific type of optical glass designed to meet the strict requirements of high-precision optical systems on material stress and optical properties. The main characteristics of this type of glass are low internal stress and high optical precision.

[0003] Traditional optical glass is usually made of a relatively single raw material composition, and it is difficult to achieve a good balance in terms of chemical stability, refractive index adjustment, and hardness. In order to increase the refractive index, some optical glasses may excessively increase the content of certain specific components, resulting in reduced chemical stability or insufficient hardness. The light transmittance of traditional optical glass may not be excellent enough, and it performs poorly in high-precision imaging applications, and cannot meet the high requirements of modern optical systems for imaging quality. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a method for preparing low-stress and high-precision optical glass to solve the problem that the light transmittance of traditional optical glass may not be excellent enough due to the excessive increase in the content of certain specific components in order to improve the refractive index, resulting in decreased chemical stability or insufficient hardness.

[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing low-stress high-precision optical glass comprises the following steps:

[0006] S1. Raw material preparation: according to the performance requirements of the required optical glass, prepare glass raw materials, the glass raw materials include dioxide pentoxide; barium oxide; aluminum oxide; sodium oxide; zinc oxide; zirconium oxide; boron trioxide; titanium dioxide or nano silicon powder;

[0007] S2. Mixing raw materials: Put the prepared glass raw materials into the mixing device, first add boron pentoxide and boron trioxide into the mixing device, then add barium oxide, aluminum oxide, sodium oxide, zinc oxide and zirconium oxide, and finally add titanium dioxide or nano silicon powder into the mixing device for mixing;

[0008] S3, melting: crushing and mixing the prepared glass raw materials, adding them into a melting container for melting, clarifying, and melting, and continuously introducing oxygen-rich air to obtain molten glass liquid;

[0009] S4, molding and annealing: select molds according to the finished products, ensure that the mold surface is smooth and free of defects to ensure the surface quality of the molded glass, add Rongtai's glass liquid into the container for cooling and molding, control the cooling speed to gradually solidify the glass, use natural cooling or cooling with a cooling device to put the molded glass products into the annealing furnace to avoid collision and damage, ensure that the glass products can be heated evenly, and the heating speed should not be too fast to avoid causing a sharp change in the internal stress of the glass. Keep it at the annealing temperature for a certain period of time to fully release the internal stress of the glass, cool it, and take out the glass after cooling;

[0010] S5, polishing: prepare and mix the polishing materials, place the glass in the polishing area for polishing, and add the mixed polishing materials into the polishing machine to polish the glass;

[0011] S6. Surface cleaning: Choose a suitable cleaning place and perform cleaning operations in a clean, dust-free, and well-ventilated environment to avoid re-contamination of the glass surface. Place the polished glass in the cleaning area of ​​the cleaning device to clean the surface of the glass. Use a compressed air spray gun to blow the glass surface to remove larger particles. Then rinse the glass with deionized water through the cleaning device to remove residual detergent and impurities. After rinsing, blow dry with liquid nitrogen to ensure that the glass surface is completely dry to avoid water stains or other problems caused by residual moisture;

[0012] S7. Coating treatment: First clean the coating equipment to ensure that the inside of the coating equipment is clean and prevent contamination of the film layer. Place the optical glass that has been surface cleaned on the sample rack of the coating equipment to ensure that the glass surface is clean, free of scratches and dust pollutants. Use high-energy ions to bombard the sputtering target and sputter the sputtering target material onto the glass substrate to form a film layer.

[0013] Preferably, the amounts of glass raw materials in S1 are: 35-50wt% phosphorus pentoxide; 20-40wt% barium oxide; 2-5wt% aluminum oxide; 2-8wt% sodium oxide; 1-4wt% zinc oxide; 1-3wt% zirconium oxide; 10-20wt% boron trioxide; and 0.5-2wt% titanium dioxide or nano silicon powder.

[0014] Preferably, in S2, the rotation speed of the mixing device is 50-200 rpm, the temperature is 30-50° C., and the mixing time is 15-25 minutes.

[0015] Preferably, in S3, the smelting container includes a corundum container or a quartz container, the melting temperature of the corundum container or the quartz container is 1400-1600°C, the melting time is 8-12 hours, the clarification temperature is 1600-1700°C, the clarification time is 1-3 hours, the oxygen concentration is 25-40%, and the ventilation flow rate is 30-50 cubic meters / hour.

[0016] Preferably, in S4, the wind speed of the cooling device is 5-20 m / s, the cooling time is 5-12 hours, the annealing device has an annealing temperature of 400-700°C, a heating rate of 1-5°C / min, a holding time of 5-10 hours, and a cooling rate of 0.5-2°C / min.

[0017] Preferably, in S5, the polishing material includes: 20-50 parts of rare earth polishing powder; 3-15 parts of organic solvent; 3-15 parts of inorganic solvent; 1-5 parts of clay; 40-80% of deionized water, the inorganic additives include 15%-25% of zirconium salt; 10%-20% of zinc nitrate; 8%-15% of zinc sulfate; 12%-22% of zinc titanate, the rare earth polishing powder includes 62-66% of cerium oxide; 34-38% of lanthanum oxide; 1-6% of praseodymium oxide, the organic additives include surfactant: 8%-15%; 5%-10% of chelating agent; 3%-8% of defoaming agent; 10%-18% of dispersant, the rotation speed of the polishing machine is 1000-3000 rpm, the downward pressure is 0.1-0.8MPa, and the injection pressure is 0.2-0.6MPa.

[0018] Preferably, in S6, the pressure of the cleaning equipment spray gun is 0.3-0.6 MPa, the nozzle diameter is 1-3 mm, the flushing pressure is 0.2-0.4 MPa, the flow rate is 5-20 L / min, the liquid nitrogen flow rate is 1-5 L / min, and the nozzle height is 10-20 cm.

[0019] Preferably, in S7, the cleaning gas pressure of the coating equipment is 0.3-0.6 MPa, the cleaning time is 15-30 minutes, the sputtering power is 500-1000 W, the sputtering pressure is 5-15 mTorr, the sputtering rate is 5-10 nm / min, and the coating material is calcium fluoride: 5%-15%; tantalum pentoxide: 5%-15%.

[0020] The present invention provides a method for preparing low-stress high-precision optical glass. It has the following beneficial effects:

[0021] 1. The present invention can improve chemical stability and adjust the refractive index through phosphorus pentoxide; barium oxide increases the refractive index; aluminum oxide increases hardness and mechanical strength. After the glass raw materials are mixed, the optical glass has high cost performance, is easy to achieve mass production, and has excellent light transmission performance. In addition, by adding nano titanium dioxide or nano silicon powder, the refractive index of the optical glass is further improved, the chemical stability is good, and it is suitable for high-precision imaging mirrors, which simplifies the optical system and improves the imaging quality.

[0022] 2. The present invention effectively reduces the stress inside the glass through annealing, combined with a specific cooling rate and holding time, so that the glass can slowly release the internal stress during the cooling process. Low-stress optical glass has higher stability and reliability, is less likely to crack or deform, and extends its service life. Low stress also helps to improve the optical uniformity of the glass, reduce optical distortion, and improve imaging quality.

[0023] 3. The present invention ensures the high precision of optical glass through coating treatment. The high-precision glass surface has high flatness and low roughness. This is due to the synergistic effect of rare earth polishing powder including cerium oxide, lanthanum oxide, praseodymium oxide and inorganic and organic additives in the polishing material, which makes the glass composition uniform and the structure dense, further prolonging the service life during use and improving the mirror refractive index. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a flow chart of the present invention; DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Embodiment 1:

[0027] Please refer to the attached Figure 1 , the embodiment of the present invention provides 1. a method for preparing low-stress high-precision optical glass, characterized in that it comprises the following steps:

[0028] S1. Raw material preparation: Prepare glass raw materials according to the performance requirements of the required optical glass. The glass raw materials include dioxide pentoxide; barium oxide; aluminum oxide; sodium oxide; zinc oxide; zirconium oxide; boron trioxide; titanium dioxide or nano silicon powder;

[0029] S2. Mixing raw materials: Put the prepared glass raw materials into the mixing device, first add boron pentoxide and boron trioxide into the mixing device, then add barium oxide, aluminum oxide, sodium oxide, zinc oxide and zirconium oxide, and finally add titanium dioxide or nano silicon powder into the mixing device for mixing;

[0030] S3, melting: crushing and mixing the prepared glass raw materials, adding them into a melting container for melting, clarifying, and melting, and continuously introducing oxygen-rich air to obtain molten glass liquid;

[0031] S4, molding and annealing: select molds according to the finished products, ensure that the mold surface is smooth and free of defects to ensure the surface quality of the molded glass, add Rongtai's glass liquid into the container for cooling and molding, control the cooling speed to gradually solidify the glass, use natural cooling or cooling with a cooling device to put the molded glass products into the annealing furnace to avoid collision and damage, ensure that the glass products can be heated evenly, and the heating speed should not be too fast to avoid causing a sharp change in the internal stress of the glass. Keep it at the annealing temperature for a certain period of time to fully release the internal stress of the glass, cool it, and take out the glass after cooling;

[0032] S5, polishing: prepare and mix the polishing materials, place the glass in the polishing area for polishing, and add the mixed polishing materials into the polishing machine to polish the glass;

[0033] S6. Surface cleaning: Choose a suitable cleaning place and perform cleaning operations in a clean, dust-free, and well-ventilated environment to avoid re-contamination of the glass surface. Place the polished glass in the cleaning area of ​​the cleaning device to clean the surface of the glass. Use a compressed air spray gun to blow the glass surface to remove larger particles. Then rinse the glass with deionized water through the cleaning device to remove residual detergent and impurities. After rinsing, blow dry with liquid nitrogen to ensure that the glass surface is completely dry to avoid water stains or other problems caused by residual moisture;

[0034] S7. Coating treatment: First clean the coating equipment to ensure that the inside of the coating equipment is clean and prevent contamination of the film layer. Place the optical glass that has been surface cleaned on the sample rack of the coating equipment to ensure that the glass surface is clean, free of scratches and dust pollutants. Use high-energy ions to bombard the sputtering target and sputter the sputtering target material onto the glass substrate to form a film layer.

[0035] In S1, the proportions of glass raw materials are: 35wt% of phosphorus pentoxide; 20wt% of barium oxide; 2wt% of aluminum oxide; 2wt% of sodium oxide; 1-4wt% of zinc oxide; 1-3wt% of zirconium oxide; 10-20wt% of boron trioxide; and 0.5-2wt% of titanium dioxide or nano silicon powder.

[0036] Phosphorus pentoxide improves chemical stability, helps improve the resistance of glass to water and acid, enhances the stability of glass in different environments, and can adjust the refractive index of glass to a certain extent to meet the needs of different optical applications. Barium oxide can significantly increase the refractive index of glass and is suitable for optical systems that require high refractive performance. It improves the chemical corrosion resistance of glass, makes the glass denser, and enhances its mechanical properties. Aluminum oxide increases the hardness of glass, making it more resistant to wear and scratches, while increasing the strength of glass and reducing the risk of breakage. It enhances the resistance of glass to water, acid and alkali, and helps control the dimensional stability of glass when the temperature changes. Sodium oxide acts as a flux to lower the melting temperature of glass, making it easier to process, increase the fluidity of glass, and improve the fluidity of glass in a molten state, which is beneficial to the forming and clarification of glass. Zinc oxide improves the chemical stability of glass and enhances the resistance of glass to Water, acid and alkali resistance, helps to improve the dimensional stability of glass, reduce the risk of breakage caused by temperature changes, adjust the refractive index and dispersion of glass, zirconium oxide makes glass have higher hardness and wear resistance, suitable for applications requiring high mechanical strength, has good resistance to chemicals such as acids and alkalis, maintains good performance at high temperatures, and reduces performance changes caused by temperature changes. Boron trioxide, as a flux, reduces the melting temperature of glass, enhances the resistance of glass to water and acid, and helps control the dimensional stability of glass when the temperature changes. Titanium dioxide has a high refractive index and can increase the optical properties of glass. Titanium dioxide has a good absorption effect on ultraviolet rays and can protect glass from damage by ultraviolet rays; Nano-silicon powder can adjust the refractive index of glass to a certain extent. Improve the color and appearance of glass: it can make the glass present a specific color or gloss.

[0037] In S2, the rotation speed of the mixing device is 50 rpm, the temperature is 30° C., and the mixing time is 15 minutes.

[0038] When the uniformly mixed raw materials enter the smelting process, the speed of 50 rpm is neither too fast to cause splashing and uneven mixing of raw materials, nor too slow to make the mixing efficiency low. The temperature of 30°C is relatively low, close to room temperature. At this temperature, the physical and chemical properties of the raw materials are relatively stable, and chemical reactions or phase changes are not easy to occur. The mixing time of 15 minutes can give the raw materials enough time to be fully mixed. During this period of time, the stirring action of the mixing device can make the raw materials move and collide continuously in all directions, gradually reaching a state of uniform mixing.

[0039] In S3, the smelting container includes a corundum container, the melting temperature of the corundum container is 1400°C, the melting time is 8 hours, the clarification temperature is 1600°C, the clarification time is 1 hour, the oxygen concentration is 25%, and the ventilation flow rate is 30 cubic meters / hour.

[0040] The melting temperature of 1400℃ can fully melt the glass raw materials. Various oxides, phosphorus pentoxide, barium oxide, aluminum oxide, etc. gradually soften and melt at this temperature to form uniform glass liquid. The melting time of 8 hours is sufficient, which can allow the glass raw materials to have enough time for heat transfer and chemical reaction. The impurities in the raw materials can gradually volatilize or react with other components to form easily discharged compounds. Long-term melting can make the composition of the glass liquid more uniform and reduce the situation of local uneven composition.

[0041] Raising the temperature to 1600℃ is helpful to discharge bubbles and remove impurities in the molten glass. At this temperature, the viscosity of the molten glass decreases, and bubbles are more likely to rise to the liquid surface and burst to discharge some refractory impurities. They can also react with other components in the molten glass at high temperatures. One hour of clarification time can allow enough time for bubbles and impurities in the molten glass to be discharged. An oxygen concentration of 25% can promote the oxidation reaction of the glass raw materials and help remove some reducing impurities.

[0042] In S4, the wind speed of the cooling device is 5 m / s, the cooling time is 5 hours, the annealing device, the annealing temperature is 400°C, the heating rate is 1°C / min, the holding time is 5 hours, and the cooling rate is 0.5°C / min.

[0043] A wind speed of 5 m / s can effectively take away the heat of the glass and accelerate the cooling process. This wind speed will not be too strong to cause excessive wind erosion or stress concentration on the glass surface. At the same time, it can also ensure cooling efficiency. During the cooling process, the cooling speed of each part of the glass is relatively consistent, reducing the internal stress caused by uneven cooling. The cooling time of 5 hours is moderate, which can gradually cool the glass from a high temperature state to near room temperature, avoiding stress and cracks caused by rapid cooling, and reducing the accumulation of residual stress. The annealing temperature of 400°C is close to the transition temperature of the glass, which can eliminate internal stress at this temperature and improve the strength and stability of the glass.

[0044] The heating rate is 1℃ / min. The slow heating rate can avoid new stress in the glass due to rapid temperature change. The holding time is 5 hours. The longer holding time can ensure that the glass can fully eliminate stress and adjust its structure at the annealing temperature. The cooling rate is 0.5℃ / min. The slow cooling rate can gradually cool the glass after annealing to avoid new stress due to rapid cooling.

[0045] In S5, the polishing materials include: 20 parts of rare earth polishing powder; 3 parts of organic solvent; 3 parts of inorganic solvent; 1 part of clay; 40% deionized water, inorganic additives include 15% zirconium salt; 10% zinc nitrate; 8% zinc sulfate; 12% zinc titanate, rare earth polishing powder includes 62% cerium oxide; 34% lanthanum oxide; 1% praseodymium oxide, organic additives include 8% surfactant; 5% chelating agent; 3% defoaming agent; 10% dispersant, the speed of the polishing machine is 1000 rpm, the down pressure is 0.1, and the injection pressure is 0.2.

[0046] Cerium oxide of rare earth polishing powder is one of the main components of rare earth polishing powder. It has high hardness and good polishing performance. It can quickly remove tiny flaws and roughness on the glass surface and make the glass surface smooth. During the polishing process, cerium oxide particles rub against the glass surface and remove the uneven parts of the surface through mechanical action. Lanthanum oxide can improve the hardness and wear resistance of the polishing powder and enhance the polishing effect. It works synergistically with cerium oxide to more effectively remove scratches and defects on the glass surface. At the same time, lanthanum oxide can also improve the dispersibility of the polishing powder, making it more evenly distributed on the glass surface during the polishing process. The content of praseodymium oxide in rare earth polishing powder is relatively small, but it can play a role in adjusting the performance of the polishing powder.

[0047] Clay can increase the viscosity and stability of the polishing liquid and prevent the precipitation of polishing powder particles. During the polishing process, clay can make the polishing powder more evenly distributed on the glass surface and improve the polishing effect;

[0048] Deionized water is one of the main components of the polishing liquid. It can dilute and disperse the polishing powder. During the polishing process, deionized water can evenly disperse the polishing powder particles on the glass surface, making it fully contact with the glass surface and improving the polishing efficiency.

[0049] Zirconium salts as inorganic additives can improve the hardness and wear resistance of glass and enhance the polishing effect. During the polishing process, zirconium salts can react with oxides on the surface of the glass to form a hard protective film to prevent the glass surface from being damaged during the polishing process. Zinc nitrate can improve the dispersibility and stability of the polishing liquid and prevent the precipitation of polishing powder particles. During the polishing process, zinc nitrate can react with oxides on the surface of the glass to form compounds that are easy to remove. Zinc sulfate can adjust the pH value of the polishing liquid to make it more suitable for glass polishing. During the polishing process, zinc sulfate can react with oxides on the surface of the glass to form compounds that are easy to remove. Zinc titanate can improve the refractive index and transparency of the glass, making the polished glass surface more beautiful. During the polishing process, zinc titanate can react with oxides on the surface of the glass to form a uniform film to improve the optical properties of the glass.

[0050] The surfactant of organic additive can reduce the surface tension of polishing liquid, making it easier for polishing powder to disperse on the glass surface. The chelating agent can form a stable complex with metal ions to prevent metal ions from contaminating the glass surface. The defoaming agent can eliminate bubbles in the polishing liquid to prevent bubbles from forming pits and defects on the glass surface. The dispersant can improve the dispersibility and stability of polishing powder and prevent the precipitation of polishing powder particles.

[0051] In S6, the pressure of the cleaning equipment spray gun is 0.3, the nozzle diameter is 1 mm, the flushing pressure is 0.2 MPa, the flow rate is 5 L / min, the liquid nitrogen flow rate is 1 L / min, and the nozzle height is 10 cm.

[0052] The pressure is 0.3MPa, which can effectively blow away larger particles of impurities on the glass surface, such as dust, fibers, etc. The pressure is neither too low to remove impurities, nor too high to damage the glass surface or embed impurities on the glass surface. For example, some particles with weak adhesion can be easily blown off the glass surface, laying a good foundation for subsequent cleaning steps; the nozzle diameter is 1 mm: a smaller nozzle diameter can produce a more concentrated airflow, which can accurately blow specific areas on the glass surface, improving the pertinence and efficiency of cleaning; the deionized water flushing pressure is 0.2MPa. This pressure can make the deionized water fully rinse the glass surface and remove residual detergent and fine impurities; the flow rate is 5L / min. The appropriate flow rate can ensure that the deionized water can cover the entire glass surface and achieve comprehensive flushing; the liquid nitrogen flow rate is 1L / min. This flow rate can make the liquid nitrogen quickly freeze and sublimate the moisture on the glass surface to ensure that the glass surface is completely dry. The moderate flow rate can effectively remove moisture, and will not cause stress or damage to the glass surface due to excessive flow rate. The nozzle height is 10cm to ensure the consistency of the drying effect. The distance will not be too close, causing the liquid nitrogen to be concentrated in a local area and causing the temperature to be too low, nor will the distance be too far, causing the effect of the liquid nitrogen to be weakened.

[0053] In S7, the cleaning gas pressure of the coating equipment is 0.3 MPa, the cleaning time is 15 minutes, the sputtering power is 500, the sputtering pressure is 5 mTorr, the sputtering rate is 5 nm / min, and the coating materials are calcium fluoride: 5%; tantalum pentoxide: 5%.

[0054] The sputtering power is 500W, which can provide enough energy for the sputtering process, so that the atoms or molecules in the sputtering target are bombarded by high-energy ions and detached from the target surface, and deposited on the glass substrate to form a film layer. The sputtering pressure is 5 mTorr. The lower sputtering pressure can make the average free path of the sputtering ions longer and the energy higher, which is beneficial to improve the quality and adhesion of the film layer. The sputtering rate is 5 nanometers / minute: this rate is relatively slow, but it can ensure that the growth process of the film layer is relatively stable, which is beneficial to control the thickness and quality of the film layer. Tantalum pentoxide can provide good protection and optical properties. Calcium fluoride has good chemical corrosion resistance and is not easy to react with other substances under normal conditions, which can maintain the stability and durability of the film layer.

[0055] The difference between the second embodiment and the first embodiment is the following steps:

[0056] In S1, the amounts of glass raw materials are: 50wt% of phosphorus pentoxide, 40wt% of barium oxide, 5wt% of aluminum oxide, 8wt% of sodium oxide, 4wt% of zinc oxide, 3wt% of zirconium oxide, 20wt% of boron trioxide, and 2wt% of titanium dioxide or nano silicon powder.

[0057] In S2, the rotation speed of the mixing device is 200 rpm, the temperature is 50° C., and the mixing time is 25 minutes.

[0058] In S3, the smelting container includes a quartz container, the melting temperature of the quartz container is 1600°C, the melting time is 12 hours, the clarification temperature is 1700°C, the clarification time is 3 hours, the oxygen concentration is 40%, and the ventilation flow rate is 50 cubic meters / hour.

[0059] In S4, the wind speed of the cooling device is 20 m / s, the cooling time is 12 hours, the annealing device, the annealing temperature is 700°C, the heating rate is 5°C / min, the holding time is 10 hours, and the cooling rate is 2°C / min.

[0060] In S5, the polishing materials include: 50 parts of rare earth polishing powder; 15 parts of organic solvent; 15 parts of inorganic solvent; 5 parts of clay; 80% deionized water, inorganic additives include 25% zirconium salt; 20% zinc nitrate; 15% zinc sulfate; 22% zinc titanate, rare earth polishing powder includes 66% cerium oxide; 38% lanthanum oxide; 6% praseodymium oxide, organic additives include 15% surfactant; 10% chelating agent; 8% defoaming agent; dispersant 18%, the polishing machine has a rotation speed of 3000 rpm, a downward pressure of 0.8 MPa, and a spray pressure of 0.6 MPa.

[0061] In S6, the pressure of the cleaning equipment spray gun is 0.6MPa, the nozzle diameter is 3mm, the flushing pressure is 0.4MPa, the flow rate is 20L / min, the liquid nitrogen flow rate is 5L / min, and the nozzle height is 20cm.

[0062] In S7, the cleaning gas pressure of the coating equipment is 0.6MPa, the cleaning time is 30 minutes, the sputtering power is 1000W, the sputtering pressure is 15 mTorr, the sputtering rate is 10 nm / min, and the coating materials are calcium fluoride: 15%; tantalum pentoxide: 15%.

[0063]

[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing low-stress high-precision optical glass, characterized in that: The following steps are involved: S1. Raw material preparation: according to the performance requirements of the required optical glass, prepare glass raw materials, the glass raw materials include dioxide pentoxide; barium oxide; aluminum oxide; sodium oxide; zinc oxide; zirconium oxide; boron trioxide; titanium dioxide or nano silicon powder; S2. Mixing raw materials: Put the prepared glass raw materials into the mixing device, first add boron pentoxide and boron trioxide into the mixing device, then add barium oxide, aluminum oxide, sodium oxide; Zinc oxide and zirconium oxide are added inside, and finally titanium dioxide or nano silicon powder is added inside for mixing; S3, melting: crushing and mixing the prepared glass raw materials, adding them into a melting container for melting, clarifying, and melting, and continuously introducing oxygen-rich air to obtain molten glass liquid; S4, molding and annealing: select molds according to the finished products, ensure that the mold surface is smooth and free of defects to ensure the surface quality of the molded glass, add Rongtai's glass liquid into the container for cooling and molding, control the cooling speed to gradually solidify the glass, use natural cooling or cooling with a cooling device to put the molded glass products into the annealing furnace to avoid collision and damage, ensure that the glass products can be heated evenly, and the heating speed should not be too fast to avoid causing a sharp change in the internal stress of the glass. Keep it at the annealing temperature for a certain period of time to fully release the internal stress of the glass, cool it, and take out the glass after cooling; S5, polishing: prepare and mix the polishing materials, place the glass in the polishing area for polishing, and add the mixed polishing materials into the polishing machine to polish the glass; S6. Surface cleaning: Choose a suitable cleaning place and perform cleaning operations in a clean, dust-free, and well-ventilated environment to avoid re-contamination of the glass surface. Place the polished glass in the cleaning area of ​​the cleaning device to clean the surface of the glass. Use a compressed air spray gun to blow the glass surface to remove larger particles. Then rinse the glass with deionized water through the cleaning device to remove residual detergent and impurities. After rinsing, blow dry with liquid nitrogen to ensure that the glass surface is completely dry to avoid water stains or other problems caused by residual moisture; S7. Coating treatment: First clean the coating equipment to ensure that the inside of the coating equipment is clean and prevent contamination of the film layer. Place the optical glass that has been surface cleaned on the sample rack of the coating equipment to ensure that the glass surface is clean, free of scratches and dust pollutants. Use high-energy ions to bombard the sputtering target and sputter the sputtering target material onto the glass substrate to form a film layer.

2. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S1, the proportions of glass raw materials are: 35-50wt% of phosphorus pentoxide; 20-40wt% of barium oxide; 2-5wt% of aluminum oxide; 2-8wt% of sodium oxide; 1-4wt% of zinc oxide; 1-3wt% of zirconium oxide; 10-20wt% of boron trioxide; and 0.5-2wt% of titanium dioxide or nano silicon powder.

3. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S2, the rotation speed of the mixing device is 50-200 rpm, the temperature is 30-50° C., and the mixing time is 15-25 minutes.

4. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S3, the smelting container includes a corundum container or a quartz container, the melting temperature of the corundum container or the quartz container is 1400-1600°C, the melting time is 8-12 hours, the clarification temperature is 1600-1700°C, the clarification time is 1-3 hours, the oxygen concentration is 25-40%, and the ventilation flow rate is 30-50 cubic meters / hour.

5. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S4, the wind speed of the cooling device is 5-20 m / s, the cooling time is 5-12 hours, the annealing device, the annealing temperature is 400-700°C, the heating rate is 1-5°C / min, the holding time is 5-10 hours, and the cooling rate is 0.5-2°C / min.

6. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S5, the polishing material includes: 20-50 parts of rare earth polishing powder; 3-15 parts of organic solvent; 3-15 parts of inorganic solvent; 1-5 parts of clay; 40-80% of deionized water, the inorganic additives include 15%-25% of zirconium salt; 10%-20% of zinc nitrate; 8%-15% of zinc sulfate; 12%-22% of zinc titanate, the rare earth polishing powder includes 62-66% of cerium oxide; 34-38% of lanthanum oxide; 1-6% of praseodymium oxide, the organic additives include surfactant: 8%-15%; 5%-10% of chelating agent; 3%-8% of defoaming agent; 10%-18% of dispersant, the rotation speed of the polishing machine is 1000-3000 rpm, the downward pressure is 0.1-0.8MPa, and the injection pressure is 0.2-0.6MPa.

7. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S6, the pressure of the cleaning equipment spray gun is 0.3-0.6MPa, the nozzle diameter is 1-3mm, the flushing pressure is 0.2-0.4MPa, the flow rate is 5-20L / min, the liquid nitrogen flow rate is 1-5L / min, and the nozzle height is 10-20cm.

8. The method for preparing low-stress high-precision optical glass according to claim 1, characterized in that: In S7, the cleaning gas pressure of the coating equipment is 0.3-0.6 MPa, the cleaning time is 15-30 minutes, the sputtering power is 500-1000 W, the sputtering pressure is 5-15 mTorr, the sputtering rate is 5-10 nm / min, and the coating material is calcium fluoride: 5%-15%; Tantalum pentoxide: 5%-15%.

Citation Information

Cited By

  • High-precision ultra-smooth optical glass and preparation method thereof

    CN120229872A

  • High-precision ultra-smooth optical glass and preparation method thereof

    CN120229872B

  • Clarifying agent for producing photovoltaic glass and preparation method thereof

    CN121426431A

  • A fining agent for producing photovoltaic glass and a method for preparing the same

    CN121426431B