Olefin polymerization termination method
By using antioxidants such as high boiling point phenol stabilizers as catalyst inactivators in olefin polymerization, the problem of selecting catalyst inactivators in the prior art is solved, and the rapid termination of polymerization and efficient production are achieved, thereby reducing the need for lowering the energy consumption and cost.
Patent Information
- Application Number
- CN202411273668.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing olefin polymerization process, the selection of catalyst deactivators has problems such as polarity mismatch, high cost, large energy consumption and complex equipment, making it difficult to effectively terminate the polymerization reaction and improve production efficiency.
Polyolefin antioxidants such as high boiling point phenol stabilizers, organophosphorus composites and lactones are used as catalyst inactivators. After the polymerization reaction is completed, the volatile components are removed in vacuo to control the length of the polymerization chain. and reduce low molecular weight polymer content.
The rapid termination of the polymerization reaction is achieved, the low molecular weight of the gel is reduced, the oxidative degradation is prevented, the production efficiency is improved, the energy consumption and cost are reduced, and the reactor pollution and heat exchanger clogging are avoided.
Smart Images

Figure BDA0005040607520000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of olefin polymerization, and in particular relates to a method for terminating olefin polymerization. Background Art
[0002] Polyolefin materials have stable physical and chemical properties, especially polyethylene PE and polypropylene PP, which are widely used in our daily lives. Polyolefins are the first in the production of synthetic polymers worldwide. In addition, polyolefins have low production costs and are less toxic than other commodity plastics, which also meets the requirements of sustainable development and green polymer chemistry.
[0003] The olefin polymerization liquid phase contains the synthesized polymer, unreacted monomers, inert hydrocarbon solvents and catalyst systems. After the polymerization reaction is completed, the industrial production process needs to be subjected to a devolatilization post-treatment to remove volatile components, such as unreacted monomers, inert hydrocarbon solvents, etc., from the polymerization liquid phase mixture. However, since the catalyst system in the system is not deactivated, the unreacted monomers can continue to undergo polymerization in the subsequent devolatilization step. As the devolatilization conditions change, the polymerization reaction will produce a series of low molecular weight polymers, which will have a greater impact on the physical properties of the polymers (melt index, molecular weight distribution, etc.) finally obtained, thereby reducing the mechanical properties of the polymers. Therefore, the polymerization reaction needs to be terminated at an appropriate time to ensure the desired molecular structure and performance. In production, terminators control the length of the polymer chain by preventing the polymerization reaction from continuing, thereby adjusting the properties of the final product. Therefore, precise polymerization control can affect the molecular weight, molecular weight distribution, melt index, mechanical properties, etc. of polyolefin products.
[0004] In the existing production technology, water or other alcohol substances are generally used as terminators, but there are many disadvantages. Patent document US2020 / 10562988 uses water and low boiling point compounds (CO 2 Or alcohol) as a catalyst deactivator. On the one hand, water and alcohols are polar solvents and have poor compatibility with non-polar polymer solutions. The prepared polyolefin has a large viscosity, and many active centers are surrounded by macromolecular polymer chains, which makes it difficult to contact with water or alcohol terminators to complete polymerization termination. On the other hand, after the introduction of water or alcohols, it will enter the reactor outlet flow, which may cause the presence of deactivators in the recovery flow, thereby causing the feed flow of the polymerization kettle to be contaminated and causing the catalyst to deactivate. Therefore, the post-treatment deashing equipment has high requirements, large energy loss, and high cost.
[0005] Patent document US2020 / 10562988 adds an antioxidant to the polymerization system in the third step after adding water as a deactivator in the second step to prevent the polymer from being oxidatively degraded during the devolatilization process. However, when the water content in the system is high, the added antioxidant is hydrolyzed, and the hydrolysis product is devolatilized and cooled by the heat exchanger, thereby crystallizing and causing the heat exchanger to become clogged. Therefore, the water content in the system needs to be less than 3ppm, resulting in a contradiction between the second and third steps.
[0006] Patent document US2011 / 0172375 uses methanol as a deactivator, and two additional separation steps are required in the deashing process, namely water-alcohol separation and subsequent drying. In addition, the use of alcohols will form hydrochloric acid, causing corrosion and scaling problems.
[0007] Patent document WO 2009 / 126277 uses sodium stearate or calcium stearate as a solid deactivating agent, but the deashing process requires more equipment to remove the solid deactivating agent, such as a drying bed, a stripping tower, an additional column, etc., which will result in greater energy loss and higher costs.
[0008] Therefore, developing an efficient, simple, and low-cost catalyst deactivator to terminate the polymerization reaction more quickly, improve the production efficiency of the polymerization process, reduce energy consumption, and reduce costs has become a technical problem that needs to be urgently solved in this field. Summary of the invention
[0009] In order to improve the above technical problems, the present invention provides the use of a polyolefin antioxidant as a catalyst deactivator for olefin polymerization reactions;
[0010] The polyolefin antioxidant has a boiling point greater than 300° C. and is selected from one or more of phenolic stabilizers, organic phosphorus compounds, lactones and hydroxylamines.
[0011] According to an embodiment of the present invention, the phenolic stabilizer includes but is not limited to tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester (antioxidant 1010), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate n-octadecyl alcohol ester (antioxidant 1076), N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine (antioxidant 1098), N,N'-bis[β -(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (antioxidant 1024), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane (antioxidant CA), 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione (antioxidant MIANOX1790), etc., one or more thereof.
[0012] According to an embodiment of the present invention, the organic phosphorus complex includes but is not limited to one or more of trinonylphenyl phosphite (antioxidant TNP), tri[2.4-di-tert-butylphenyl]phosphite (antioxidant 168), bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (antioxidant 626), triphenyl phosphite (antioxidant TPP), etc.
[0013] According to an embodiment of the present invention, the lactone and hydroxylamine antioxidants include but are not limited to one or more of distearyl thiodipropionate (antioxidant DSTP), distearyl thiodipropionate (antioxidant DSTDP), dilauryl thiodipropionate (antioxidant DLTP), pentaerythritol stearate (antioxidant PETS), 2,2'-thiodiethyl bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (antioxidant 1035), pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant 412S), triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate (antioxidant 245), bis-octylamine (antioxidant FS042), etc.
[0014] In an exemplary embodiment, the polyolefin antioxidant is selected from one or more of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076), dilauryl thiodipropionate (antioxidant DLTP), tris[2.4-di-tert-butylphenyl]phosphite (antioxidant 168), pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant 412S), N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] hydrazine (antioxidant 1024) and bis-octylamine (antioxidant FS042).
[0015] When the polyolefin antioxidant is selected from two or more types, each antioxidant can be in any proportion. For example, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester (antioxidant 1076) and dilauryl thiodipropionate (antioxidant DLTP) and tris[2.4-di-tert-butylphenyl] phosphite (antioxidant 168) mixed in any proportion, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester (antioxidant 1076) and dilauryl thiodipropionate (antioxidant DLTP) mixed in any proportion, Pentaerythritol tetrakis (3-laurylthiopropionate) (Antioxidant 412S) and N,N'-bis [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl] hydrazine (Antioxidant 1024), pentaerythritol tetrakis (3-laurylthiopropionate) (Antioxidant 412S), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (Antioxidant 1076) and tris [2,4-di-tert-butylphenyl] phosphite (Antioxidant 168) mixed in any proportion.
[0016] According to an embodiment of the present invention, the polyolefin antioxidant is added after the polymerization stage is completed (ie, a polymerization system is formed), for example, the polyolefin antioxidant is added to the polymerization system at the outlet flow of the polymerization reactor.
[0017] According to an embodiment of the present invention, the olefin includes but is not limited to one or more of ethylene, propylene, and α-olefin.
[0018] According to an embodiment of the present invention, the olefin polymerization includes but is not limited to ethylene homopolymerization, propylene homopolymerization, copolymerization of ethylene and α-olefin, or copolymerization of propylene and α-olefin.
[0019] According to an embodiment of the present invention, the α-olefin is selected from C 3 -C 20 One or more olefins, for example, selected from C 4 Olefins, C 5 Olefins, C 6 Olefins, C 7 Olefins, C 8 Olefins (such as 1-octene), C 9 Olefins, C 10 Olefins, C 11 Olefins, C 12 Olefins, C 13 Olefins, C 14 Olefins, C 15 Olefins, C 16 Olefins, C 17 Olefins, C 18 Olefins, C 19 One or more of olefins.
[0020] According to an embodiment of the present invention, the catalyst includes a main catalyst and a co-catalyst;
[0021] The main catalyst is selected from one or more of the following (1)-(4):
[0022] (1) supported Ziegler-Natta catalysts, wherein the carrier is a magnesium chloride carrier, an alkoxy carrier, a silica gel carrier and / or a composite carrier; (2) metallocene catalysts, such as one or more of rac-dimethylsilylbis(1-indenyl)zirconium dichloride, dimethylsilyl(tert-butylamino)tetramethylcyclopentadienylzirconium dichloride, (η(5)-(indenyl)dimethylsilyl(tert-butyl)amide)titanium dichloride, rac-dimethylsilyl-bis(2-methyl-4-phenylindenyl)zirconium dichloride, etc.; (3) non-metallocene catalysts; (4) composite catalysts;
[0023] The co-catalyst is selected from one or more of the following (a)-(c):
[0024] (a) Alkyl aluminoxane, such as one or more of methyl aluminoxane (MAO), ethyl aluminoxane (EAO), butyl aluminoxane (BAO) or composite alkyl aluminoxane; (b) organic boron compound, such as one or more of triphenyl carbon tetrakis (pentafluorophenyl) borate, triphenylmethyl tetrafluoroborate, triethylmethylammonium tetrafluoroborate, tri(o-tolyl)phosphine tetrafluoroborate, etc.; (c) supported multi-nuclear co-catalyst.
[0025] In one embodiment, the main catalyst is a metallocene catalyst, and the co-catalyst is an organic boron compound or an alkylaluminoxane.
[0026] According to an embodiment of the present invention, the amount of the polyolefin antioxidant added is at least equivalent to the molar amount of the main catalyst, for example, the molar ratio of the polyolefin antioxidant to the main catalyst is not less than 50:1, 100:1, 200:1, 300:1 or 400:1, such as 500:1, 550:1 or 600:1.
[0027] According to an embodiment of the present invention, the amount of the polyolefin antioxidant added is at most 0.5% of the total mass of the polyolefin.
[0028] The present invention also provides a method for terminating olefin polymerization, comprising: adding the above polyolefin antioxidant to a polymerization system formed by an olefin polymerization reaction, for example, adding the polyolefin antioxidant to the polymerization system at the outlet flow of a polymerization reactor.
[0029] According to an embodiment of the present invention, the polymerization system is a solution polymerization system or a slurry polymerization system, for example, a polymer solution.
[0030] According to an embodiment of the present invention, the method comprises: adding a catalyst and an olefin into an inert hydrocarbon solvent for polymerization to form a polymerization system, for example, to form a polymer solution;
[0031] The catalyst and olefin are both as defined above.
[0032] According to an embodiment of the present invention, the inert hydrocarbon solvent is selected from C 5 -C 30 Saturated hydrocarbons, C 5 -C 30 Alicyclic hydrocarbons, C 6 -C 30 Aromatic hydrocarbons, C 3 -C 20 Saturated heterocyclic hydrocarbon or paraffin oil, or a mixture of the aforementioned solvents; preferably C 5 -C 10 A saturated hydrocarbon is, for example, n-hexane.
[0033] According to an embodiment of the present invention, the conditions for olefin polymerization include at least one of the following conditions: the polymerization temperature is 60-200°C, the hydrogen partial pressure is 0.001-0.5MPa, the ethylene partial pressure is 0.1-5MPa, the propylene partial pressure is 0.5-5MPa, the gaseous olefin partial pressure in α-olefin is 0.1-5MPa, the reaction time is 0.5h-5h, and the molar ratio of the main catalyst to the co-catalyst is 1:(0.1-200).
[0034] According to an embodiment of the present invention, the polyolefin antioxidant is added in the form of a solution, such as dissolving the polyolefin antioxidant in the inert hydrocarbon solvent to form a solution, for example, a 5-100 g / L solution. The polyolefin antioxidant can be used as a catalyst deactivator to deactivate the catalyst.
[0035] The above method further comprises removing volatile components from the polymerization system in which the catalyst has been deactivated by vacuum.
[0036] According to an embodiment of the present invention, the volatile components include one or more of unreacted raw materials (unreacted monomers), oligomers with low polymerization degree (such as dimers, trimers, etc.), organic solvents, catalyst residues, etc.
[0037] In an exemplary embodiment, the olefin polymerization termination method comprises the following steps:
[0038] a) adding one or more olefins into an inert hydrocarbon solvent and polymerizing them under the action of a catalyst to obtain a polymer solution;
[0039] b) adding a polyolefin antioxidant as a catalyst deactivator at the outlet flow of the polymerization reactor to deactivate the polymerization catalyst;
[0040] c) removing volatile components from the polymer solution in which the polymerization catalyst has been deactivated under vacuum.
[0041] The present invention also provides an olefin polymerization method, comprising the above olefin polymerization termination method.
[0042] According to an embodiment of the present invention, in the prepared polyolefin, the content of low molecular weight polymers (such as dimers, trimers, etc.) is less than 3.5 wt%, preferably less than 2 wt%, and further preferably less than 1.5 wt%.
[0043] According to an embodiment of the present invention, the low molecular weight polymer refers to a polymer with a weight average molecular weight of less than 1,000.
[0044] Beneficial Effects
[0045] The present invention adopts one or more composite polyolefin antioxidants such as high-boiling-point (greater than 300° C.) phenol stabilizers, organic phosphorus compounds, lactones and hydroxylamines as catalyst deactivators, and adds antioxidants to the outlet flow of the polymerization reactor, thereby effectively terminating the polymerization reaction, controlling the length of the polymerization chain, and reducing the content of gel low molecular weight polymers to ensure the required molecular structure and performance, and can prevent the polymer from being oxidized and degraded during the devolatilization process. The process adopts a high-boiling-point antioxidant as a catalyst deactivator, which will not enter the reactor again with the recovery flow like water components, will not pollute the feed flow of the reactor, and can also prevent the heat exchanger from being blocked by the decomposition products of the antioxidant, allowing the monomers separated from the polymerization product downstream of the polymerization reactor to be recycled back to the reactor, so that polyolefins can be produced continuously and stably for a long time, improve the production efficiency of the polymerization process, reduce energy consumption, and reduce costs. Therefore, the problem of catalyst deactivation in the polyolefin process to be solved by the present invention can be achieved.
[0046] Cost-effectively recover unreacted monomers separated from the polymer downstream of the polymerization reactor and return them to the reactor, while ensuring that the feed inlet is not contaminated by deactivators. DETAILED DESCRIPTION
[0047] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0048] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0049] Example 1
[0050] 890mL of n-hexane, 290mL of 1-octene and 0.3mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 115°C, and the ethylene pressure in the polymerization kettle is raised to 3.4MPa. 0.5μmol of rac-dimethylsilylbis(1-indenyl)zirconium dichloride main catalyst and 2μmol of triphenylcarbon tetrakis(pentafluorophenyl)borate cocatalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 1.54mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.4MPa. The polymerization temperature is set to 115°C. After 30 minutes of reaction, 20 mL of 8 g / L β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester (antioxidant 1076) n-hexane solution (molar ratio to the main catalyst is 600:1) was added to the outlet flow of the polymerization reactor as a catalyst deactivator, and the temperature was raised to 170 ° C for 4 hours. Turn off the ethylene inlet switch and the kettle heating switch, then cool to room temperature, and then open the polymerization kettle after depressurizing to normal pressure. Cool down to room temperature again, and then open the polymerization kettle after depressurizing to normal pressure. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, the polymer is dried to constant weight, which is the obtained product, a total of 238.0 g.
[0051] Example 2
[0052] 890mL of n-hexane, 290mL of 1-octene and 0.3mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 115°C, and the ethylene pressure in the polymerization kettle is raised to 3.4MPa. 0.5μmol of rac-dimethylsilylbis(1-indenyl)zirconium dichloride main catalyst and 2μmol of N,N-dimethylaniliniumtetrakis(pentafluorophenyl)borate cocatalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 1.54mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.4MPa. The polymerization temperature is set to 115°C. After 30 minutes of reaction, add 25mL of 6g / L dilauryl thiodipropionate (antioxidant DLTP) n-hexane solution (molar ratio to the main catalyst is 600:1) as a catalyst deactivator, and heat to 170°C for 4h. Turn off the ethylene inlet switch and the kettle heating switch, cool to room temperature, then depressurize the polymerization kettle to normal pressure and open the kettle. Cool to room temperature again, then depressurize the polymerization kettle to normal pressure and open the kettle. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, dry the polymer to constant weight, which is the product obtained, a total of 203.8g.
[0053] Example 3
[0054] 890mL of n-hexane, 290mL of 1-octene and 0.3mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 115°C, and the ethylene pressure in the polymerization kettle is raised to 3.4MPa. 0.5μmol of rac-dimethylsilylbis(1-indenyl)zirconium dichloride main catalyst and 2μmol of triphenylcarbon tetrakis(pentafluorophenyl)borate cocatalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 1.54mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.4MPa. The polymerization temperature is set to 115°C. After 30 minutes of reaction, 20 mL of a 10 g / L mixed n-hexane solution of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076), dilauryl thiodipropionate (antioxidant DLTP) and tris[2.4-di-tert-butylphenyl]phosphite (antioxidant 168) was added as a catalyst deactivator, and the temperature was raised to 170°C for 4 hours. The ethylene inlet switch and the kettle heating switch were turned off, and the temperature was lowered to room temperature, and then the polymerization kettle was depressurized to normal pressure and the kettle was opened. The temperature was lowered to room temperature, and then the polymerization kettle was depressurized to normal pressure and the kettle was opened. The polymer was taken out and terminated with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, the polymer was dried to constant weight, which was the obtained product, a total of 184.2 g.
[0055] Example 4
[0056] 750mL of n-hexane, 410mL of 1-octene and 2.4mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 120°C, and the ethylene pressure in the polymerization kettle is raised to 3.7MPa. 4μmol of dimethylsilyl (tert-butylamino) tetramethylcyclopentadienyl zirconium dichloride main catalyst and 8μmol of triphenylcarbon tetrakis (pentafluorophenyl) borate co-catalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 2.17mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.7MPa. The polymerization temperature is set to 120°C. After 30 minutes of reaction, add 30 mL of 50 g / L tris[2.4-di-tert-butylphenyl]phosphite (antioxidant 168) in n-hexane (molar ratio to the main catalyst is 600:1) as a catalyst deactivator, and heat to 170°C for 4 hours. Turn off the ethylene inlet switch and the kettle heating switch, cool to room temperature, then depressurize the polymerization kettle to normal pressure and open the kettle. Cool to room temperature again, then depressurize the polymerization kettle to normal pressure and open the kettle. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, dry the polymer to constant weight, which is the obtained product, a total of 89.2 g.
[0057] Example 5
[0058] 750mL of n-hexane, 410mL of 1-octene and 2.4mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 120°C, and the ethylene pressure in the polymerization kettle is raised to 3.7MPa. 4μmol of dimethylsilyl (tert-butylamino) tetramethylcyclopentadienyl zirconium dichloride main catalyst and 8μmol of triphenylcarbon tetrakis (pentafluorophenyl) borate co-catalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 2.17mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.7MPa. The polymerization temperature is set to 120°C. After 30 minutes of reaction, 30 mL of a mixed n-hexane solution of 50 g / L β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076) and dilauryl thiodipropionate (antioxidant DLTP) was added as a catalyst deactivator, and the temperature was raised to 170 ° C for 4 hours. Turn off the ethylene inlet switch and the kettle heating switch, then cool to room temperature, and then open the polymerization kettle after depressurizing it to normal pressure. Cool down to room temperature again, and then open the polymerization kettle after depressurizing it to normal pressure. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, the polymer was dried to constant weight, which is the obtained product, a total of 95.7 g.
[0059] Example 6
[0060] 750 mL of n-hexane, 410 mL of 1-octene and 2.4 mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 118°C, and the ethylene pressure in the polymerization kettle is raised to 3.6 MPa. 4 μmol of (η(5)-(indenyl)dimethylsilyl(tert-butyl)amide)titanium dichloride main catalyst and 8 μmol of triphenylcarbon tetrakis(pentafluorophenyl)borate co-catalyst are fully dissolved in 20 mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200 mL, and the concentration of 1-octene is 2.17 mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.6 MPa. The polymerization temperature is set to 118°C. After 30 minutes of reaction, add 30 mL of a mixed n-hexane solution of pentaerythritol tetra(3-laurylthiopropionate) (antioxidant 412S) and N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (antioxidant 1024) at a concentration of 50 g / L as a catalyst deactivator, and heat to 170 ° C for 4 hours. Turn off the ethylene inlet switch and the kettle heating switch, cool to room temperature, then depressurize the polymerization kettle to normal pressure and open the kettle. Cool to room temperature again, then depressurize the polymerization kettle to normal pressure and open the kettle. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, dry the polymer to constant weight, which is the obtained product, a total of 73.9 g.
[0061] Example 7
[0062] 890mL of n-hexane, 290mL of 1-octene and 0.3mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 120°C, and the ethylene pressure in the polymerization kettle is raised to 3.4MPa. 0.5μmol of rac-dimethylsilyl-di(2-methyl-4-phenylindenyl) zirconium dichloride main catalyst and 2μmol of triphenylcarbon tetrakis(pentafluorophenyl) borate cocatalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 1.54mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.4MPa. The polymerization temperature is set to 120°C. After 30 minutes of reaction, 30 mL of a mixed n-hexane solution of 50 g / L pentaerythritol tetra(3-laurylthiopropionate) (antioxidant 412S), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate n-octadecyl alcohol (antioxidant 1076) and tris[2.4-di-tert-butylphenyl]phosphite (antioxidant 168) was added as a catalyst deactivator, and the temperature was raised to 170°C for 4 hours. The ethylene inlet switch and the kettle heating switch were turned off, and the temperature was lowered to room temperature, and then the polymerization kettle was depressurized to normal pressure and the kettle was opened. The temperature was lowered to room temperature, and then the polymerization kettle was depressurized to normal pressure and the kettle was opened. The polymer was taken out and terminated with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, the polymer was dried to constant weight, which was the obtained product, a total of 200.5 g.
[0063] Example 8
[0064] 900mL of n-hexane, 280mL of 1-octene and 0.2mmol of triisobutylaluminum (molar ratio to the main catalyst is 400:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 120°C, and the ethylene pressure in the polymerization kettle is raised to 3.4MPa. 0.5μmol of rac-dimethylsilyl-bis(2-methyl-4-phenylindenyl) zirconium dichloride main catalyst and 150μmol of methylaluminoxane (MAO) are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 1.49mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.4MPa. The polymerization temperature is set to 120°C. After 30 minutes of reaction, add 15mL of 10g / L dioctylamine (antioxidant FS042) n-hexane solution (molar ratio to main catalyst is 550:1) as a catalyst deactivator, and heat to 170°C for 4h. Turn off the ethylene inlet switch and the kettle heating switch, cool to room temperature, then depressurize the polymerization kettle to normal pressure and open the kettle. Cool to room temperature again, then depressurize the polymerization kettle to normal pressure and open the kettle. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtration, dry the polymer to constant weight, which is the obtained product, a total of 188.5g.
[0065] Comparative Example 1
[0066] 890mL of n-hexane, 290mL of 1-octene and 0.3mmol of triisobutylaluminum (molar ratio to the main catalyst is 600:1) are introduced into the polymerization kettle at room temperature. The polymerization kettle is heated to 115°C, and the ethylene pressure in the polymerization kettle is raised to 3.4MPa. 0.5μmol of rac-dimethylsilylbis(1-indenyl)zirconium dichloride main catalyst and 2μmol of triphenylcarbon tetrakis(pentafluorophenyl)borate cocatalyst are fully dissolved in 20mL of n-hexane to form an activated catalyst solution (total volume of the polymerization system is 1200mL, and the concentration of 1-octene is 1.54mol / L). Subsequently, the activated catalyst solution is quickly injected into the polymerization kettle to initiate polymerization, and the ethylene gas switch is turned on to replenish ethylene at any time, so that the pressure of the polymerization kettle is maintained at 3.4MPa. The polymerization temperature is set to 115°C. After 30 minutes of reaction, the temperature is raised to 170°C and maintained for 4h. Turn off the ethylene inlet switch and the kettle heating switch, cool down to room temperature, then release the pressure of the polymerization kettle to normal pressure and open the kettle. Take out the polymer and terminate it with an acid-alcohol solution (ethanol: hydrochloric acid = 9:1). After filtering, dry the polymer to constant weight, which is the obtained product, a total of 175.0g.
[0067] The catalyst activities and polymer physicochemical properties of each example and comparative example are shown in Table 1.
[0068] Table 1 Catalyst activity and polymer physicochemical properties
[0069]
[0070] Note: The low molecular weight polymer content in the table refers to the mass percentage of the part with weight average molecular weight less than 1000 in the total molecular weight.
[0071] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. Application of polyolefin antioxidant as catalyst deactivator for olefin polymerization reaction, characterized in that: The polyolefin antioxidant has a boiling point greater than 300° C. and is selected from one or more of phenolic stabilizers, organic phosphorus compounds, lactones and hydroxylamines.
2. The use according to claim 1, wherein The phenolic stabilizers include but are not limited to pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076), N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine (antioxidant 1098), N,N'-bis[β-(3,5 One or more of: 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane (antioxidant CA), and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione (antioxidant MIANOX1790); And / or, the organophosphorus compound includes, but is not limited to, one or more of trisnonylphenyl phosphite (antioxidant TNP), tris[2,4-di-tert-butylphenyl]phosphite (antioxidant 168), bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (antioxidant 626), and triphenyl phosphite (antioxidant TPP); And / or, the lactone and hydroxylamine antioxidants include but are not limited to one or more of distearyl thiodipropionate (antioxidant DSTP), distearyl thiodipropionate (antioxidant DSTDP), dilauryl thiodipropionate (antioxidant DLTP), pentaerythritol stearate (antioxidant PETS), 2,2'-thiodiethyl bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (antioxidant 1035), pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant 412S), triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate (antioxidant 245), and bis-octylamine (antioxidant FS042).
3. The use according to claim 1, wherein: The olefins include but are not limited to one or more of ethylene, propylene, and α-olefins; Alternatively, the olefin polymerization includes but is not limited to ethylene homopolymerization, propylene homopolymerization, copolymerization of ethylene and α-olefin, or copolymerization of propylene and α-olefin.
4. The use according to claim 3, wherein: The α-olefin is selected from C3-C 20 One or more olefins, for example, selected from C4 olefins, C5 olefins, C6 olefins, C7 olefins, C8 olefins (such as 1-octene), C9 olefins, C 10 Olefins, C 11 Olefins, C 12 Olefins, C 13 Olefins, C 14 Olefins, C 15 Olefins, C 16 Olefins, C 17 Olefins, C 18 Olefins, C 19 One or more olefins.
5. The use according to claim 1, wherein The catalyst includes a main catalyst and a co-catalyst; The main catalyst is selected from one or more of the following (1)-(4): (1) supported Ziegler-Natta catalysts, wherein the support is a magnesium chloride support, an alkoxy support, a silica gel support and / or a composite support; (2) metallocene catalysts, such as one or more of rac-dimethylsilylbis(1-indenyl)zirconium dichloride, dimethylsilyl(tert-butylamino)tetramethylcyclopentadienylzirconium dichloride, (η(5)-(indenyl)dimethylsilyl(tert-butyl)amide)titanium dichloride, and rac-dimethylsilyl-bis(2-methyl-4-phenylindenyl)zirconium dichloride; (3) non-metallocene catalysts; (4) composite catalysts; The co-catalyst is selected from one or more of the following (a)-(c): (a) an alkylaluminoxane, such as one or more of methylaluminoxane (MAO), ethylaluminoxane (EAO), butylaluminoxane (BAO) or a composite alkylaluminoxane; (b) an organic boron compound, such as one or more of triphenylcarbon tetrakis(pentafluorophenyl)borate, triphenylmethyl tetrafluoroborate, triethylmethylammonium tetrafluoroborate, tri(o-tolyl)phosphine tetrafluoroborate, etc.; (c) a supported multinuclear cocatalyst.
6. The use according to any one of claims 1 to 5, wherein The amount of the polyolefin antioxidant added is at least equivalent to the molar amount of the main catalyst, and the maximum amount of the polyolefin antioxidant added is 0.5% of the total mass of the polyolefin.
7. A method for terminating olefin polymerization, characterized in that: The following steps are involved: a) adding one or more olefins into an inert hydrocarbon solvent and polymerizing them under the action of a catalyst to obtain a polymer solution; b) adding a polyolefin antioxidant as a catalyst deactivator at the outlet of the polymerization reactor to deactivate the polymerization catalyst; c) removing volatile components from the polymer solution in which the polymerization catalyst has been deactivated under vacuum; The polyolefin antioxidant has a boiling point greater than 300° C. and is selected from one or more of phenolic stabilizers, organic phosphorus compounds, lactones and hydroxylamines.
8. The method for terminating olefin polymerization according to claim 7, wherein: The one or more polyolefin antioxidants in step b) are dissolved in the same solvent as the polymerization system to prepare a 5-100 g / L solution; And / or, the volatile components in step c) include unreacted raw materials (unreacted monomers), oligomers with low polymerization degree (such as dimers, trimers, etc.), organic solvents, and catalyst residues.
9. The method for terminating olefin polymerization according to claim 7, wherein: In step a), the inert hydrocarbon solvent is selected from C5-C 30 Saturated hydrocarbons, C5-C 30 Alicyclic hydrocarbons, C6-C 30 Aromatic hydrocarbons or C3-C 20 saturated heterocyclic hydrocarbons or paraffin oil or a mixed solvent thereof.
10. The method for terminating olefin polymerization according to claim 7, wherein The polymerization system is a solution polymerization system or a slurry polymerization system; And / or, the conditions for olefin polymerization include at least one of the following conditions: polymerization temperature is 60-200°C, hydrogen partial pressure is 0.001-0.5 MPa, ethylene partial pressure is 0.1-5 MPa, propylene partial pressure is 0.5-5 MPa, gaseous olefin partial pressure in α-olefin is 0.1-5 MPa, reaction time is 0.5h-5h, and the molar ratio of main catalyst to co-catalyst is 1:(0.1-200).
Citation Information
Cited By
Phosphite antioxidant based on bio-based lignin phenol as well as preparation method and application of phosphite antioxidant
CN119613446A
Phosphite antioxidant based on bio-based lignin phenol and preparation method and application thereof