Polyurethane polishing layer of chemical mechanical polishing pad, preparation method and application of polyurethane polishing layer and polishing pad

By using isocyanate prepolymer and functional filler polyurethane polishing layer, the problem of Particle number and scratch risk during the polishing process is solved, and the density uniformity and polishing efficiency of polishing layer are improved, meeting the high-precision needs of complex semiconductor devices.

CN119039558APending Publication Date: 2024-11-29WANHUA CHEM GRP ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411226866.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When manufacturing complex semiconductor devices, it is difficult to achieve a balance between reducing the number of Particles during the polishing process and maintaining the polishing rate and scratch risk, and the uneven density distribution of the polishing layer affects the polishing effect.

Method used

Polyurethane polished layer prepared by reaction of isocyanate prepolymer, polyether polyol and small molecule polyol, and combined with specific curing agents such as 3,5 -Dimethylthiotoluenediamine, controls the uniform distribution of density and hardness of the polishing layer.

Benefits of technology

It is achieved that while maintaining a moderate polishing rate, the number of parts after polishing is significantly reduced, the polishing quality and efficiency are improved, the density and hardness uniformity of the polishing layer are ensured, and the risk of scratches is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024866740000191
    Figure BDA0005024866740000191
  • Figure BDA0005024866740000192
    Figure BDA0005024866740000192
  • Figure BDA0005024866740000201
    Figure BDA0005024866740000201
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical mechanical polishing pads, and particularly relates to a polyurethane polishing layer of a chemical mechanical polishing pad, a preparation method and application of the polyurethane polishing layer and the polishing pad. The polyurethane polishing layer is a product prepared from an isocyanate prepolymer, a curing agent and a functional filler; the isocyanate prepolymer is a product prepared by reacting isocyanate, polyether polyol and optional micromolecular polyol of which the relative molecular weight is less than or equal to 500; the curing agent is a diamine compound; the functional filler comprises expanded polymer hollow-core microspheres and inorganic nonmetal powder; the particle size of the inorganic nonmetal powder is larger than 1 micrometer and smaller than 6 micrometers. The polishing layer has the high and stable polishing rate, meanwhile, density distribution is uniform, uniformity is good, and the polishing quality of the polishing pad is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical mechanical polishing pads, and in particular relates to a polyurethane polishing layer of a chemical mechanical polishing pad, a preparation method and application thereof, and a polishing pad. Background Art

[0002] Semiconductor production typically includes some chemical mechanical planarization (CMP) process. In each CMP process, a polishing pad together with a polishing liquid (e.g., a polishing slurry containing an abrasive or an active liquid without an abrasive) is used to remove excess material in a planing manner or to maintain its flatness in order to subsequently receive a new layer. The stack of these layers is combined in a manner to form an integrated circuit.

[0003] The manufacturing of these semiconductor devices is becoming increasingly complex due to the demand for devices with higher operating speeds, lower leakage currents, and lower power consumption. In terms of device structure, this means that the geometry of the parts (features) needs to be finer and the metallization level needs to be increased. These increasingly stringent device design requirements have led to the use of copper plating operations in conjunction with new dielectric materials with lower dielectric constants. The reduced physical properties (usually associated with low-k and ultra-low-k materials) combined with the increase in device complexity have increased the requirements for CMP consumables such as polishing pads and polishing slurries. Specifically, low-k and ultra-low-k dielectric materials tend to have lower mechanical strength and poorer adhesion than conventional dielectric materials, making planarization operations more difficult.

[0004] In addition, as the size of integrated circuit parts decreases, defects such as particles caused by CMP become a bigger problem. In addition, the reduction in the thickness of integrated circuit films requires that acceptable configurations be provided for the wafer substrate while improving defects. These configuration requirements place higher requirements on flatness, concavity, erosion, and the number of particles (referring to the number of residual particles on the wafer surface).

[0005] In the traditional polishing pad preparation method, most of them use polyols and polyisocyanates to react to prepare isocyanate-terminated urethane prepolymers, which are then foamed or pore-formed, and mixed with polyamines to solidify into the required polyurethane polishing pads. In this type of system, no filler is generally added (except for the expanded hollow microspheres of foamed or pore-formed polymers), so the polishing pad has a certain viscosity (the main body of the polishing pad is a polyurethane elastomer, which is a polymer material and therefore has a certain viscoelasticity), which can easily lead to the adhesion of polishing particles (such as SiO2 or CeO2, etc.) in the polishing liquid during the polishing process, resulting in an increase in the number of particles. In the selection of curing agents, 3,3'-dichloro-4,4'-diphenylmethane diamine (also known as MOCA) is generally preferred for strength and wear resistance considerations. However, the elasticity of the polishing pad prepared by it is slightly poor, and the viscosity is outstanding, which can also easily lead to an increase in the number of particles during the polishing process. In addition, 3,3'-dichloro-4,4'-diphenylmethanediamine (MOCA) requires a high temperature of about 110°C-120°C when used. The high temperature of the curing agent plus the reaction heat generated by the reaction of the urethane prepolymer and the curing agent will cause the entire process of the polishing pad to react violently and the gel time will be short. Finally, the formation of bubbles in the polishing pad will be uneven, resulting in uneven hardness and density distribution of the polishing pad, affecting the polishing effect.

[0006] For advanced process technologies, such as those with feature sizes of 28nm and below, polishing pads are required to have lower defects and fewer particles.

[0007] It is well known in the art that the use of polyurethane with a low viscosity molecular structure can effectively reduce defects such as particles generated during polishing. However, reducing the viscosity of polyurethane generally requires increasing hardness, which in turn changes the polishing rate and increases the risk of scratches during polishing. Therefore, how to achieve an ideal balance between fewer particles, polishing rate and scratch risk is an important issue that needs to be paid attention to in the research and development of polishing pads. Summary of the invention

[0008] The purpose of the present invention is to achieve a balance between fewer particles, polishing rate and scratch risk. The present invention provides a polyurethane polishing layer of a chemical mechanical polishing pad and a preparation method and a polishing pad. The polishing layer has a high and stable polishing rate and also makes the semiconductor substrate have fewer particles after polishing. In addition, the density distribution of the polishing layer is uniform and uniform, which improves the polishing quality of the polishing pad.

[0009] In order to achieve the above-mentioned purpose, the present invention provides the following technical solutions:

[0010] In a first aspect, a polyurethane polishing layer of a chemical mechanical polishing pad is provided, which is a product obtained by reacting an isocyanate prepolymer, a curing agent and a functional filler; the isocyanate prepolymer is a product obtained by reacting an isocyanate, a polyether polyol and an optional small molecule polyol having a relative molecular weight of less than or equal to 500 (e.g., 10, 20, 40, 50, 80, 100, 200, 300, 400);

[0011] The curing agent is a diamine compound;

[0012] The functional filler includes expanded polymer hollow microspheres and inorganic non-metallic powder; the particle size of the inorganic non-metallic powder is greater than 1 micron and less than 6 microns (for example, 1.5 microns, 2 microns, 2.5 microns, 3 microns, 3.5 microns, 4 microns, 4.5 microns, 5 microns, 5.5 microns), preferably 2-4 microns.

[0013] According to the polyurethane polishing layer provided by the present invention, in some embodiments, based on the total mass of each component, the components and their contents in the reaction raw materials of the isocyanate prepolymer are as follows:

[0014] Isocyanate, 30-50wt% (e.g., 32wt%, 34wt%, 35wt%, 36wt%, 38wt%, 40wt%, 42wt%, 45wt%, 48wt%), preferably 30-40wt%;

[0015] Polyether polyol, 40-60wt% (e.g., 42wt%, 44wt%, 45wt%, 46wt%, 48wt%, 50wt%, 52wt%, 55wt%, 58wt%), preferably 50-60wt%;

[0016] Small molecule polyol, 0-10wt% (e.g., 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 4wt%, 5wt%, 6wt%, 8wt%), preferably 5wt%-10wt%.

[0017] According to the polyurethane polishing layer provided by the present invention, in some embodiments, the polyether polyol is a homopolyether obtained by ring-opening polymerization of tetrahydrofuran under the initiation of a cationic initiator, with a functionality of 2 and a number average molecular weight of 650-3000 (for example, 700, 800, 900, 1000, 1200, 1400, 1500, 1600, 1800, 2000, 2500, 2800), preferably with a number average molecular weight of 1000-2000.

[0018] Polytetrahydrofuran polyol itself contains ether bonds and a considerable number of regularly arranged methylene groups. The polyurethane material prepared from it has high modulus and strength, as well as excellent elasticity, wear resistance, dynamic mechanical properties and low-temperature flexibility. In addition, it also has certain properties that polyester polyurethane materials cannot achieve, especially good water resistance. As we all know, the polishing liquid used in the polishing process is mostly water, and it also has a certain acidity or alkalinity, so it is particularly important for the polishing pad itself to have excellent hydrolysis resistance.

[0019] The polytetrahydrofuran polyol used in the present invention can be prepared according to existing processes, or directly adopt commercial products, for example, but not limited to, PolyTHF 1000 of BASF of Germany and Terathane 1000 of INVISTA of the United States.

[0020] In some embodiments, the isocyanate is selected from the group consisting of methylene bis-4,4'-cyclohexyl diisocyanate, cyclohexyl diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, tetramethylene-1,4-diisocyanate, 1,6-hexamethylene diisocyanate, dodecane-1,12-diisocyanate, cyclobutane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane, methylcyclohexene diisocyanate, hexamethylene diisocyanate, 2,4,4-diisocyanate, and triisocyanates. -Triisocyanate of trimethyl-1,6-hexane diisocyanate, ethylene diisocyanate, 2,2,4-trimethylhexane diisocyanate, 2,2,4-trimethylhexane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, uretdione-modified MDI, one or more of carbodiimide-modified MDI, preferably selected from toluene diisocyanate, more preferably a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (wherein the mass fraction of 2,4-toluene diisocyanate is 80%, the mass fraction of 2,6-toluene diisocyanate is 20%, also known as TDI-80).

[0021] In some embodiments, the small molecule polyol is selected from one or more of diethylene glycol, dipropylene glycol and tripropylene glycol, preferably diethylene glycol (diethylene glycol).

[0022] Adding a certain amount of small molecule polyols when synthesizing isocyanate prepolymers can effectively reduce the content of free isocyanate monomers in the prepolymer, making the molecular structure of the prepolymer more regular; at the same time, small molecule polyols can also increase the polarity of the hard segment molecular structure in the polyurethane molecular structure, making the hard segment structure easier to aggregate to form micro-regions, increasing the degree of phase separation between the soft segment molecular structure and the hard segment molecular structure in the polyurethane molecular chain, so that the comprehensive performance of the polyurethane polishing layer is improved. In some preferred embodiments, compared with other small molecule polyols, diethylene glycol has better flexibility due to the ether bond contained in the molecular structure, and the elastic properties of the prepared polyurethane polishing layer are better.

[0023] Although the polyurethane polishing layer generated by the reaction of existing small molecule diamine compounds with isocyanate prepolymers has high mechanical strength, its reaction activity with isocyanate prepolymers is very high and the gel time is short. For the polyurethane polishing layer of chemical mechanical polishing, the curing reaction of isocyanate prepolymers with such small molecule diamines is relatively fast, the gel time is relatively short, and the reaction exotherm is relatively high, which will not only cause the expanded polymer hollow microspheres as functional fillers to be unevenly dispersed in the polymer, but also cause them to continue to expand due to heat inside the polishing layer, increase the diameter of the microspheres, and even break. These two undesirable effects will cause the density and hardness of the final polishing layer to be uneven, which will in turn affect the final polishing effect, such as inconsistent removal rate, increased scratches, and increased defective rate.

[0024] In some embodiments, the diamine compound is 3,5-dimethylthiotoluenediamine. The molecular structure of 3,5-dimethylthiotoluenediamine contains two methylthio groups, which rotate inward, so that the polyurethane material prepared by it increases flexibility and elasticity; in addition, 3,5-dimethylthiotoluenediamine is used as a curing agent, and the gel time when it reacts with isocyanate prepolymer is prolonged, the reaction exotherm is reduced, the reaction process is smoother, and the expanded polymer hollow microspheres are more evenly dispersed in the polishing layer and are not easy to break. The prepared polishing layer will be more uniform (for example, the density and hardness of the polishing layer are uniform), which is conducive to improving the final polishing effect.

[0025] The curing agent used in the present invention can be prepared according to existing processes, or directly adopt commercially available products, such as Ethacure 300 from Albemarle Corporation of the United States, Addolinkb 1705 from Rhein Chemie of Germany, and the like.

[0026] Herein, the isocyanate prepolymer can be prepared by the prior art in the art, and is not particularly limited thereto. For example, a process can be adopted: isocyanate, polyether polyol and small molecule polyol are reacted at 75-80° C. for 1-3 hours to obtain a prepolymer with a desired NCO content.

[0027] In some embodiments, the expanded hollow polymer microspheres include a capsule structure having an outer wall of polyacrylonitrile copolymer and a low-boiling-point alkane gas having a boiling point of 50° C. or less filled in the capsule structure.

[0028] In some embodiments, the low boiling point alkane gas is selected from one or more of isobutane, n-pentane and dimethylpropane.

[0029] In the present invention, the expanded polymer hollow microspheres used can be obtained from commercial channels, such as 551DE40d42 and 461DET40d25 from Nouryon of the Netherlands and FN-80SDE from Matsumoto of Japan.

[0030] In some embodiments, the inorganic non-metallic powder is selected from one or more of calcium carbonate, wollastonite, talc, calcium sulfate and boron nitride. In some preferred embodiments, the inorganic non-metallic powder is boron nitride (e.g., boron nitride with a particle size of 2-4 microns). Boron nitride can be prepared according to existing processes, or commercially available products can be directly used, such as TW02 of Shandong Jingyi New Materials Co., Ltd., BN-AB of Weifang Zhuoyu New Materials Technology Co., Ltd., etc.

[0031] As a lubricant, boron nitride can reduce the friction coefficient of polyurethane, increase its lubricity, and reduce the viscosity of the polishing layer. When adding it to the polishing layer system, there are certain requirements for its particle size, which cannot be too large or too small. If the particle size of boron nitride is too small, it will have almost no lubricating effect on the polishing layer, and there will be no significant improvement in the number of particles on the surface of the polishing substrate after polishing. If the particle size of boron nitride is too large, it will destroy the microphase separation structure of the polishing layer matrix resin polyurethane, reduce the hardness of the polishing layer, and ultimately lead to a decrease in the polishing rate during the polishing process.

[0032] According to the polyurethane polishing layer provided by the present invention, in some embodiments, the density (referring to the overall density) of the polyurethane polishing layer is 0.6 g / cm 3 -0.9g / cm 3 (For example, 0.62 g / cm 3 , 0.65g / cm 3 , 0.7g / cm 3 , 0.72g / cm 3 , 0.74g / cm 3 , 0.75g / cm 3 、0.78g / cm 3 , 0.8g / cm 3 , 0.82g / cm 3 , 0.84g / cm 3 , 0.85g / cm 3 , 0.86g / cm 3, 0.88g / cm 3 ), preferably 0.75 g / cm 3 -0.85g / cm 3 ; Its Shore hardness is 50D-65D (for example, 52D, 54D, 55D, 56D, 58D, 60D, 62D, 64D), preferably 55D-65D.

[0033] The polyurethane polishing layer of the present invention has good elasticity and uniform density distribution. Under the premise of ensuring a moderate and stable polishing rate, the number of particles in the polishing substrate is significantly reduced after polishing, so that the polishing quality and polishing efficiency are taken into consideration and balanced.

[0034] In a second aspect, a method for preparing the polyurethane polishing layer as described above is provided, comprising the following steps:

[0035] a) mixing isocyanate, polyether polyol and optional small molecule polyol for prepolymerization to obtain an isocyanate prepolymer, wherein the NCO content of the isocyanate prepolymer is preferably 6wt%-10wt% (e.g., 7wt%, 8wt%, 9wt%);

[0036] b) uniformly mixing the inorganic non-metallic powder and the isocyanate prepolymer to obtain a mixture containing the inorganic non-metallic powder;

[0037] c) uniformly mixing the curing agent, the mixture containing inorganic non-metallic powder and the polymer expanded hollow microspheres to obtain a gelled mixture;

[0038] d) pouring the gelled mixture into a mold, demoulding, and then secondary vulcanizing the mixture to obtain the polyurethane polishing layer.

[0039] According to the preparation method provided by the present invention, in some embodiments, in step a), the prepolymerization reaction temperature is 75-80°C (eg, 76°C, 78°C), and the prepolymerization reaction time is 1-3h (eg, 1.5h, 2h, 2.5h).

[0040] The preparation process of the isocyanate prepolymer in step a) can be a conventional operation in the art. For example, first weigh the required mass of isocyanate in a reaction container and maintain its temperature at about 60°C, then add the polyether polyol at about 60°C to the isocyanate in batches or dropwise, then add the small molecule polyol at about 40°C to the mixture of isocyanate and polyether polyol in batches or dropwise, then increase the reaction temperature to 75-80°C, react at constant temperature for 1-3 hours, take a sample to measure the NCO% content, and vacuum degassing and discharge the material after reaching the preset value.

[0041] In step b) and step c), the mixing operation process and equipment can be conventional operations in the art and will not be described in detail here. In this article, the inorganic non-metallic powder and the polymer expanded hollow microspheres are added to the system in steps, which can ensure that the inorganic non-metallic powder and the polymer expanded hollow microspheres are evenly dispersed in the polishing layer. If the inorganic non-metallic powder and the polymer expanded hollow microspheres are added to the system at the same time and mixed, due to the large difference in density between the two raw materials, the inorganic non-metallic powder and the polymer expanded hollow microspheres will be unevenly dispersed in the polishing layer, which will lead to uneven density of the polishing layer.

[0042] In some embodiments, step d) is to pour the gelled mixture into a mold at 80°C-85°C (e.g., 82°C, 84°C), demold after gelling for 15-20 minutes (e.g., 16 minutes, 18 minutes), and then post-vulcanize it at 100°C-120°C (e.g., 105°C, 110°C, 115°C) for 16-20 hours (e.g., 17 hours, 18 hours, 19 hours).

[0043] In some embodiments, the stoichiometric ratio (molar ratio) of NH2 in the curing agent to NCO in the isocyanate prepolymer is 90%-125% (e.g., 95%, 100%, 105%, 110%, 115%, 120%), preferably 90%-110%. In the preparation process of the polyurethane polishing layer of the chemical mechanical polishing pad, when the isocyanate prepolymer reacts with the curing agent, if the stoichiometric ratio of NH2:NCO is too high, the cross-linked structure in the polyurethane polishing layer will increase, the hardness of the polishing layer will be too high, and the number of scratches on the semiconductor substrate will increase during the polishing process, reducing the polishing quality; on the contrary, if the stoichiometric ratio of NH2:NCO is too low, the cross-linked structure in the polyurethane polishing layer will be insufficient, the hardness of the polishing layer will be low, the removal rate during the polishing process will decrease, and the polishing efficiency will decrease.

[0044] In some embodiments, based on the total mass of the isocyanate prepolymer and the curing agent, the amount of the polymer expanded hollow microspheres is 1-3wt% (e.g., 1.2wt%, 1.4wt%, 1.5wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.8wt%), and the amount of the inorganic non-metallic powder is 1-3wt% (e.g., 1.2wt%, 1.4wt%, 1.5wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.8wt%). Boron nitride itself has a low friction coefficient, so it has a certain lubricity to the substrate. In the process of preparing the polishing layer, by adding boron nitride and controlling its amount, the friction coefficient of the polyurethane can be effectively reduced, its lubricity can be increased, and the viscosity of the polishing layer can be reduced, thereby reducing the chance of the polishing layer adhering to the polishing particles during the polishing process, and finally reducing the number of particles on the surface of the polished substrate after polishing.

[0045] In a third aspect, there is provided a use of the polyurethane polishing layer as described above or the polyurethane polishing layer prepared by the preparation method as described above in a polishing pad.

[0046] Herein, the application process and process conditions of the polyurethane polishing layer in the polishing pad may be conventional choices in the art and will not be described in detail here.

[0047] In a fourth aspect, a polishing pad is provided, which includes the polyurethane polishing layer as described above or the polyurethane polishing layer prepared by the preparation method as described above.

[0048] The polishing pad may include, for example, a substrate and a polishing layer adapted to polish the substrate. Herein, the composition and preparation process of the polishing pad including the polyurethane polishing layer may be conventional operations in the art and will not be described in detail here.

[0049] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:

[0050] The present invention controls the cross-linking structure in the polyurethane polishing layer appropriately, so that the removal rate during the polishing process is moderate. In addition, the polishing layer prepared by the chemical mechanical polishing pad of the present invention can reduce the number of particles on the surface of the polished substrate after polishing by at least 40% (up to 60%) while ensuring that its polishing rate is moderate and stable, and because the curing agent is selected preferentially, the gel time of the early material system is prolonged, so that the functional filler and the expanded polymer hollow microspheres are dispersed more evenly in the entire material system, thereby making the micropores in the polyurethane polishing layer evenly distributed, and the density of different positions of the polishing layer remains highly consistent, and finally making the storage and transportation of the polishing liquid during the polishing process stable, so that the uniformity and consistency of the polishing are good, and the polishing quality is improved. Finally, the polishing layer prepared by the chemical mechanical polishing pad of the present invention achieves a balance between polishing quality and polishing efficiency. DETAILED DESCRIPTION

[0051] In order to understand the technical features and content of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. For those who do not specify specific conditions in the embodiments, they are carried out according to normal conditions or the conditions recommended by the manufacturer.

[0052] Sources of raw materials used:

[0053] TDI-80: a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (the mass fraction of 2,4-toluene diisocyanate is 80%, the mass fraction of 2,6-toluene diisocyanate is 20%), NCO content ≥ 48.0%, Wanhua Chemical Group Co., Ltd.

[0054] PolyTHF 1000, polytetrahydrofuran polyether polyol with hydroxyl value of 106.9-118.1 mgKOH / g and functionality of 2, BASF AG;

[0055] DEG (diethylene glycol, also known as diethylene glycol), purity ≥99%, Sinopec Shanghai Petrochemical Co., Ltd.;

[0056] DPG (dipropylene glycol), purity ≥99%, Huntsman Company, USA;

[0057] Ethacure 300 (3,5-dimethylthiotoluenediamine, commonly known as E-300), amine value 9.4-9.6mmol / g, purity ≥99.0%, Albemarle, Germany;

[0058] MOCA (3,3'-dichloro-4,4'-diphenylmethanediamine), amine value 7.4-7.6mmol / g, Suzhou Xiangyuan Special Fine Chemical Co., Ltd.;

[0059] Expancel 551DE40d42 (expanded polymer hollow microspheres), pore diameter 30-50 microns, average diameter 40 microns, density 42±4 kg / m 3 , Nouryon, Netherlands;

[0060] TW02 (boron nitride powder), purity 99.3%, particle size 2 microns, tap density 0.15-0.25 g / cm 3 , Shandong Jingyi New Materials Co., Ltd.;

[0061] BN-AA (boron nitride powder) purity> 99%, particle size is 1 micron, Tap density (tapped density) is 0.2-0.4g / cm 3 , Weifang Zhuoyu New Material Technology Co., Ltd.;

[0062] BN-AB (boron nitride powder) purity> 99%, particle size is 4 microns, Tap density (tapped density) is 0.2-0.4g / cm 3 , Weifang Zhuoyu New Material Technology Co., Ltd.;

[0063] TW06-H (boron nitride powder), purity 99.7%, particle size 6 microns, Tap density (tapped density) 0.40-0.60 g / cm 3 , Shandong Jingyi New Materials Co., Ltd.;

[0064] The percentages in the following examples and comparative examples are percentages by mass and the parts are parts by mass.

[0065] The detection method is described as follows:

[0066] (1) Overall density of the polishing layer: Weigh the mass m of the entire polishing layer and measure the volume v of the polishing layer. The value of m / v is the overall density of the polishing layer.

[0067] (2) Density of the center of the polishing layer: Take a sample (circular) from the center of the polishing layer, weigh its mass m, and measure its volume v. The value of m / v is the density of the center of the polishing layer.

[0068] (3) Edge density of polishing layer: Take a sample (rectangle) from the edge of the polishing layer, weigh its mass m, and measure its volume v. The value of m / v is the edge density of the polishing layer.

[0069] (4) Polishing rate of polishing layer:

[0070] Polishing conditions: polishing pressure is 1.5 psi, polishing disc and polishing head speed is 87 / 93 rpm, polishing liquid is CuSlurry (11 times diluted, pH is 6-7), polishing pad correction wheel is 3M A165, polishing liquid flow rate is 250 ml / min, polishing machine is E460E / 12 300 mm chemical mechanical planarization system;

[0071] A stopwatch was used to count the use time of the polishing layer, and a Four Dimensions four-point detector (333A) was used to measure the thickness of 81 test points on the copper film. The copper polishing rate RR was determined by calculating the average difference based on the measurement results.

[0072] (5) Number of particles in the polishing layer: The SP5 topography detector is used to detect the particle size of the Cu wafer surface. The topography detector can automatically identify the number of particles on the entire wafer surface. The detection is performed before and after polishing to determine the removal and residual status of particles in the polishing layer.

[0073] Example 1

[0074] The preparation method of the polyurethane polishing layer is:

[0075] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A1 having an NCO% of 8.0 wt%;

[0076] (2) Weighing 3 parts of powdered boron nitride TW02 with a particle size of 2 μm, adding it to 100 parts of the isocyanate prepolymer A1 prepared above and mixing them evenly to obtain a mixture B1 containing an inorganic non-metallic powder;

[0077] (3) 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) were weighed and added to 103 parts of the mixture B1 containing inorganic non-metallic powder prepared above, and then 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine) were added, wherein the stoichiometric ratio (molar ratio) of NH2:NCO was 90%; the reaction materials were mixed uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and poured into a mold at 80°C, gelled at room temperature for 20 minutes, and then demolded, and then post-cured at 110°C for 16 hours to obtain a polyurethane polishing layer N1.

[0078] Example 2

[0079] The preparation method of the polyurethane polishing layer is:

[0080] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A2 having an NCO% of 8.0 wt %;

[0081] (2) Weighing 3 parts of powdered boron nitride BN-AB with a particle size of 4 μm, adding it to 100 parts of the isocyanate prepolymer A2 prepared above and mixing them evenly to obtain a mixture B2 containing an inorganic non-metallic powder;

[0082] (3) Weigh 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to 103 parts of the mixture B2 containing inorganic non-metallic powder prepared above, then add 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 90%; mix the reaction materials uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N2.

[0083] Example 3

[0084] The preparation method of the polyurethane polishing layer is:

[0085] (1) 40.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 52.0 parts of PolyTHF 1000 (polytetramethylene glycol) and 8.0 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A3 having an NCO% of 9.0 wt %;

[0086] (2) Weighing 3.2 parts of powdered boron nitride TW02 with a particle size of 2 μm, adding it to 100 parts of the isocyanate prepolymer A3 prepared above and mixing them evenly to obtain a mixture B3 containing an inorganic non-metallic powder;

[0087] (3) 2.3 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) were weighed and added to 103.2 parts of the mixture B3 containing inorganic non-metallic powder prepared above, and then 20.7 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine) were added, wherein the stoichiometric ratio (molar ratio) of NH2:NCO was 90%; the reaction materials were mixed uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and poured into a mold at 80°C, gelled at room temperature for 20 minutes, and then demolded, and then post-cured at 110°C for 16 hours to obtain a polyurethane polishing layer N3.

[0088] Example 4

[0089] The preparation method of the polyurethane polishing layer is:

[0090] (1) 40.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 52.0 parts of PolyTHF 1000 (polytetramethylene glycol) and 8.0 parts of DE (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A4 having an NCO% of 9.0 wt %;

[0091] (2) Weighing 3.2 parts of boron nitride powder BN-AB with a particle size of 4 μm, adding it to 100 parts of the isocyanate prepolymer A4 prepared above and mixing them evenly to obtain a mixture B4 containing inorganic non-metallic powder;

[0092] (3) Weigh 2.3 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to 103.2 parts of the mixture B4 containing inorganic non-metallic powder prepared above, then add 20.7 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 90%; mix the reaction materials uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N4.

[0093] Example 5

[0094] The preparation method of the polyurethane polishing layer is:

[0095] (1) 37.6 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 53.8 parts of PolyTHF 1000 (polytetramethylene furan polyether polyol) and 8.6 parts of DPG (dipropylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A5 having an NCO% of 8.0 wt %;

[0096] (2) Weigh 3 parts of powdered boron nitride TW02 with a particle size of 2 μm, add it to 100 parts of the isocyanate prepolymer A5 prepared above, and mix them evenly to obtain a mixture B5 containing inorganic non-metallic powder;

[0097] (3) 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) were weighed and added to 103 parts of the mixture B5 containing inorganic non-metallic powder prepared above, and then 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine) were added, wherein the stoichiometric ratio (molar ratio) of NH2:NCO was 90%; the reaction materials were mixed uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and poured into a mold at 80°C, gelled at room temperature for 20 minutes, and then demolded, and then post-cured at 110°C for 16 hours to obtain a polyurethane polishing layer N5.

[0098] Example 6

[0099] The preparation method of the polyurethane polishing layer is:

[0100] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate with a mass fraction of 80% and 2,6-toluene diisocyanate with a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A6 with an NCO% of 8.0 wt%;

[0101] (2) Weighing 3 parts of powdered boron nitride TW02 with a particle size of 2 μm, adding it to 100 parts of the isocyanate prepolymer A6 prepared above and mixing them evenly to obtain a mixture B6 containing an inorganic non-metallic powder;

[0102] (3) Weigh 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to 103 parts of the mixture B6 containing inorganic non-metallic powder prepared above, then add 22.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 110%; mix the reaction materials uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N6.

[0103] Example 7

[0104] The preparation method of the polyurethane polishing layer refers to Example 1, except that the amount of powdered boron nitride TW02 with a particle size of 2 microns added in step (2) is replaced by 1.8 parts; the remaining steps are the same as Example 1; and the polyurethane polishing layer N7 is obtained.

[0105] Comparative Example 1

[0106] The preparation method of the polyurethane polishing layer is:

[0107] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A8 having an NCO% of 8.0 wt %;

[0108] (2) Weigh 3 parts of powdered boron nitride TW02 with a particle size of 2 μm, add it to 100 parts of the isocyanate prepolymer A8 prepared above, and mix them evenly to obtain a mixture B8 containing inorganic non-metallic powder;

[0109] (3) Weigh 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to 103 parts of the mixture B7 containing inorganic non-metallic powder prepared above, then add 22.9 parts of curing agent MOCA (3,3'-dichloro-4,4'-diphenylmethanediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 90%; mix the reaction materials evenly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N8.

[0110] Comparative Example 2

[0111] The preparation method of the polyurethane polishing layer is:

[0112] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A9 having an NCO% of 8.0 wt%;

[0113] (2) Weighing 3 parts of powdered boron nitride BN-AA with a particle size of 1 μm, adding them to 100 parts of the isocyanate prepolymer A9 prepared above and mixing them evenly to obtain a mixture B9 containing an inorganic non-metallic powder;

[0114] (3) Weigh 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to 103 parts of the mixture B8 containing inorganic non-metallic powder prepared above, then add 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 90%; mix the reaction materials uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N9.

[0115] Comparative Example 3

[0116] The preparation method of the polyurethane polishing layer is:

[0117] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A10 having an NCO% of 8.0 wt %;

[0118] (2) Weighing 3 parts of powdered boron nitride TW06-H with a particle size of 6 μm, adding it to 100 parts of the isocyanate prepolymer A10 prepared above and mixing them evenly to obtain a mixture B10 containing an inorganic non-metallic powder;

[0119] (3) 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) were weighed and added to 103 parts of the mixture B9 containing inorganic non-metallic powder prepared above, and then 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine) were added, wherein the stoichiometric ratio (molar ratio) of NH2:NCO was 90%; the reaction materials were mixed uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and poured into a mold at 80°C, gelled at room temperature for 20 minutes, and then demolded, and then post-cured at 110°C for 16 hours to obtain a polyurethane polishing layer N10.

[0120] Comparative Example 4

[0121] The preparation method of the polyurethane polishing layer is:

[0122] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A11 having an NCO% of 8.0 wt %;

[0123] (2) Weighing 4 parts of boron nitride powder TW02 with a particle size of 2 μm, adding it to 100 parts of the isocyanate prepolymer A11 prepared above and mixing them evenly to obtain a mixture B11 containing an inorganic non-metallic powder;

[0124] (3) 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) were weighed and added to 104 parts of the mixture B10 containing inorganic non-metallic powder prepared above, and then 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine) were added, wherein the stoichiometric ratio (molar ratio) of NH2:NCO was 90%; the reaction materials were mixed uniformly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and poured into a mold at 80°C, gelled at room temperature for 20 minutes, and then demolded, and then post-cured at 110°C for 16 hours to obtain a polyurethane polishing layer N11.

[0125] Comparative Example 5

[0126] The preparation method of the polyurethane polishing layer is:

[0127] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A12 having an NCO% of 8.0 wt %;

[0128] (2) Weighing 1 part of boron nitride powder TW02 with a particle size of 2 μm, adding it to 100 parts of the isocyanate prepolymer A12 prepared above and mixing them evenly to obtain a mixture B12 containing an inorganic non-metallic powder;

[0129] (3) Weigh 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to 101 parts of the mixture B11 containing inorganic non-metallic powder prepared above, then add 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 90%; mix the reaction materials evenly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N12.

[0130] Comparative Example 6

[0131] The preparation method of the polyurethane polishing layer is:

[0132] (1) 38.0 parts of TDI-80 (2,4-toluene diisocyanate having a mass fraction of 80% and 2,6-toluene diisocyanate having a mass fraction of 20%), 54.4 parts of PolyTHF 1000 (polytetramethylene glycol) and 7.6 parts of DEG (diethylene glycol) were mixed and reacted at 75° C. for 2 hours, and then the obtained reactant was subjected to vacuum degassing treatment to obtain an isocyanate prepolymer A13 having an NCO% of 8.0 wt %;

[0133] (2) Weigh 2.2 parts of expanded polymer hollow microspheres (Expancel 551DE40d42) and add them to the prepolymer A13 prepared above, then add 18.5 parts of curing agent Ethacure 300 (3,5-dimethylthiotoluenediamine), wherein the stoichiometric ratio (molar ratio) of NH2:NCO is 90%; mix the reaction materials evenly at a mixing temperature of 55°C and a rotation speed of 3800 r / min, and pour them into a mold at 80°C, gel at room temperature for 20 minutes, then demold, and then perform secondary vulcanization at 110°C for 16 hours to obtain a polyurethane polishing layer N13.

[0134] Table 1 Performance test results of polyurethane polishing layer or polishing pad

[0135]

[0136] Table 2 Performance test of polyurethane polishing layer or polishing pad

[0137]

[0138]

[0139] The polyurethane polishing layer prepared in each embodiment has good elasticity and uniform density distribution. Under the premise of ensuring a moderate and stable polishing rate, the number of particles in the polishing substrate is significantly reduced after polishing, so that the polishing quality and polishing efficiency are taken into account and balanced.

[0140] In Comparative Example 1, when MOCA (3,3'-dichloro-4,4'-diphenylmethanediamine) is selected as a curing agent to react with an isocyanate prepolymer, the curing reaction is too fast and the gel time is too short, which not only causes uneven dispersion of the expanded polymer hollow microspheres, but also causes them to continue to expand due to heat inside the polishing layer, increase the diameter of the microspheres, or even rupture; this will cause uneven density distribution or hardness of the final polishing layer, thereby affecting the final polishing effect.

[0141] Although boron nitride was added in Comparative Example 2-3, the particle size thereof was not within an appropriate range, and the polishing quality or polishing efficiency of the obtained polishing layer could not be improved.

[0142] Although boron nitride was added in Comparative Examples 4-5, its amount was not controlled within an appropriate range, and the polishing quality or polishing efficiency of the obtained polishing layer could not be improved. In Comparative Example 6, no boron nitride was added, and the number of particles on the surface of the polished substrate after polishing could not be reduced.

[0143] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the spirit of the present invention.

Claims

1. A polyurethane polishing layer of a chemical mechanical polishing pad, which is a product obtained by an isocyanate prepolymer, a curing agent and a functional filler; characterized in that: The isocyanate prepolymer is a product obtained by reacting isocyanate, polyether polyol and an optional small molecule polyol with a relative molecular weight of less than or equal to 500; The curing agent is a diamine compound; The functional filler comprises expanded polymer hollow microspheres and inorganic non-metallic powder; the particle size of the inorganic non-metallic powder is greater than 1 micron and less than 6 microns, preferably 2-4 microns.

2. The polyurethane polishing layer according to claim 1, characterized in that Based on the total mass of each component, the components and their contents in the reaction raw materials of the isocyanate prepolymer are as follows: Isocyanate, 30-50wt%, preferably 30-40wt%; Polyether polyol, 40-60wt%, preferably 50-60wt%; Small molecule polyol, 0-10wt%, preferably 5wt%-10wt%.

3. The polyurethane polishing layer according to claim 1 or 2, characterized in that: The polyether polyol is a homopolyether obtained by ring-opening polymerization of tetrahydrofuran under the initiation of a cationic initiator, with a functionality of 2 and a number average molecular weight of 650-3000, preferably a number average molecular weight of 1000-2000; The isocyanate is selected from methylenebis-4,4'-cyclohexyl diisocyanate, cyclohexyl diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, tetramethylene-1,4-diisocyanate, 1,6-hexamethylene diisocyanate, dodecane-1,12-diisocyanate, cyclobutane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, 1-isocyanate-3,3,5-trimethyl-5-isocyanate methylcyclohexane, methylcyclohexene di ...cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,3-diiso One or more of isocyanate, triisocyanate of hexamethylene diisocyanate, triisocyanate of 2,4,4-trimethyl-1,6-hexane diisocyanate, ethylene diisocyanate, 2,2,4-trimethyl hexamethylene diisocyanate, 2,2,4-trimethyl hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, uretdione-modified MDI, and carbodiimide-modified MDI, preferably selected from toluene diisocyanate, more preferably a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.

4. The polyurethane polishing layer according to any one of claims 1 to 3, characterized in that The small molecule polyol is selected from one or more of diethylene glycol, dipropylene glycol and tripropylene glycol, preferably diethylene glycol.

5. The polyurethane polishing layer according to any one of claims 1 to 4, characterized in that The diamine compound is 3,5-dimethylthiotoluenediamine.

6. The polyurethane polishing layer according to any one of claims 1 to 5, characterized in that The expanded polymer hollow microspheres include a capsule structure with a polyacrylonitrile copolymer as an outer wall and a low-boiling-point alkane gas with a boiling point of less than or equal to 50° C. filled in the capsule structure; preferably, the low-boiling-point alkane gas is selected from one or more of isobutane, n-pentane and dimethylpropane; The inorganic non-metallic powder is selected from one or more of calcium carbonate, wollastonite, talc, calcium sulfate and boron nitride, preferably boron nitride.

7. The polyurethane polishing layer according to any one of claims 1 to 6, characterized in that The density of the polyurethane polishing layer is 0.6 g / cm 3 -0.9g / cm 3 , preferably 0.75 g / cm 3 -0.85g / cm 3 ; Its Shore hardness is 50D-65D, preferably 55D-65D.

8. The method for preparing a polyurethane polishing layer according to any one of claims 1 to 7, characterized in that: The steps include: a) mixing isocyanate, polyether polyol and optional small molecule polyol for prepolymerization to obtain isocyanate prepolymer, preferably the isocyanate prepolymer has an NCO content of 6wt%-10wt%; b) uniformly mixing the inorganic non-metallic powder and the isocyanate prepolymer to obtain a mixture containing the inorganic non-metallic powder; c) uniformly mixing the curing agent, the mixture containing inorganic non-metallic powder and the polymer expanded hollow microspheres to obtain a gelled mixture; d) pouring the gelled mixture into a mold, demoulding, and then secondary vulcanizing the mixture to obtain the polyurethane polishing layer; Preferably, in step a), the prepolymerization temperature is 75-80° C., and the prepolymerization time is 1-3 h; Preferably, in step d), the gelled mixture is poured into a mold at 80° C.-85° C., demoulded after gelling for 15-20 minutes, and then post-cured at 100° C.-120° C. for 16-20 hours.

9. The preparation method according to claim 8, characterized in that: The stoichiometric ratio of NH2 in the curing agent to NCO in the isocyanate prepolymer is 90%-125%, preferably 90%-110%; Based on the total mass of the isocyanate prepolymer and the curing agent, the amount of the polymer expanded hollow microspheres is 1-3wt%, and the amount of the inorganic non-metallic powder is 1-3wt%.

10. Use of the polyurethane polishing layer according to any one of claims 1 to 7 or the polyurethane polishing layer prepared by the preparation method according to any one of claims 8 to 9 in a polishing pad.

11. A polishing pad, characterized in that: The polyurethane polishing layer comprises the polyurethane polishing layer as described in any one of claims 1 to 7 or the polyurethane polishing layer prepared by the preparation method as described in any one of claims 8 to 9.

Citation Information

Cited By

  • Polishing pad and preparation method and application thereof

    CN121870630A