High-heat-resistance self-cooling energy-storage insulated cable material and preparation method thereof

By using alumina in energy storage cable materials, the synergy between silica composite materials and phase change heat storage materials, the cable is rapidly cooled at high temperature and stable operation is achieved, and the stability and durability of existing energy storage cable materials are solved. The problem of insufficient performance improves the heat resistance and service life of the cable.

CN119039682APending Publication Date: 2024-11-29SUZHOU IND PARK YIJIA NANO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177166.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing energy storage cable materials have a great risk of heating and short circuit when facing special conditions such as current overload, resulting in degradation of insulation performance, accelerated aging, insufficient stability and durability, which limits its large-scale application.

Method used

Matrix resin composed of polyethylene, polyvinyl chloride and polyether etherketone is used, and alumina and silica composite materials are added as inorganic high heat resistance fillers, and phase change heat storage materials are mixed to quickly cool down and energy storage through energy conversion. , improve the heat resistance and stability of the cable.

Benefits of technology

It realizes rapid cooling of cables at high temperatures and stable operation at low temperatures, extends the service life of the cable, improves the stability and durability of the cables, reduces the aging speed, and increases the temperature range and performance stability of the system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011017720000061
    Figure BDA0005011017720000061
  • Figure BDA0005011017720000071
    Figure BDA0005011017720000071
  • Figure BDA0005011017720000072
    Figure BDA0005011017720000072
Patent Text Reader

Abstract

The invention provides a high-heat-resistance self-cooling energy storage insulated cable material which comprises the following components in parts by weight: 100 parts of matrix resin, 20-30 parts of inorganic high-heat-resistance filler, 10-15 parts of a phase change heat storage material, 5-10 parts of a cross-linking agent, 1-3 parts of an antioxidant, 2-5 parts of a plasticizer, 1-3 parts of a stabilizer and 1-3 parts of stearic acid, wherein the inorganic high-heat-resistance filler comprises aluminum oxide, and the aluminum oxide interacts with the phase change heat storage material, so that the stability and durability of the cable material are improved. The cable material disclosed by the invention can be rapidly cooled in an energy conversion form, has an energy storage effect, and has good stability and durability and more stable cable performance while the operating temperature range of a system is increased, so that the performance of the system is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrical insulation materials, and in particular to a highly heat-resistant self-cooling energy storage insulating cable material and a preparation method thereof. Background Art

[0002] The global demand for energy storage is becoming increasingly important in today's society, and is particularly important in power systems. Energy storage systems can improve the stability and resilience of the power grid, especially in the face of sudden load fluctuations or power system failures, and can quickly respond and provide backup power. With the rapid development of electricity today, the widespread application of energy storage cables has become a trend.

[0003] Today's energy storage cables are mostly made of copper as conductor, heat-resistant 90℃ polyvinyl chloride PVC insulation or heat-resistant 125℃ low-smoke halogen-free flame-retardant cross-linked polyolefin XLPO insulation. The temperature resistance grades of the cables are 90℃ and 125℃. There is still a great risk of heating and short circuit in dealing with special circumstances such as current overload, which leads to a decrease in cable insulation performance, accelerated aging, and limited system performance.

[0004] The above problems can be solved by self-cooling the cable. For example, by improving the heat dissipation performance of the cable through structural design, or by adding a protective layer to maximize the working environment of the conductor, the stability and durability of the cable during use can be increased. However, the self-cooling effect of the cable in this structural design method is poor, and the cost of raw materials is high. The damage to the cable has been great for a long time, and there are great potential risks. For another example, by designing the components of the cable material, the cable can release heat during use to achieve the purpose of self-cooling. However, the cable material prepared by this method currently has a slow self-cooling effect, and the performance under low temperature conditions cannot be guaranteed. The stability and durability cannot meet the requirements, which limits its popularity in large-scale applications. Summary of the invention

[0005] The purpose of the present invention is to provide a high heat-resistant self-cooling energy storage insulating cable material and a preparation method thereof in order to address the problems of poor stability and durability of existing self-cooling cable materials. The cable material can quickly cool down by energy conversion and has an energy storage function. While increasing the operating temperature range of the system, it has good stability and durability, and the cable performance is more stable, thereby ensuring the performance of the system.

[0006] According to the first aspect of the present invention, a high heat-resistant self-cooling energy storage insulating cable material is provided, which comprises the following components by weight: 100 parts of base resin, 20-30 parts of inorganic high heat-resistant filler, 10-15 parts of phase change heat storage material, 5-10 parts of cross-linking agent, 1-3 parts of antioxidant, 2-5 parts of plasticizer, 1-3 parts of stabilizer, and 1-3 parts of stearic acid;

[0007] Among them, the inorganic high heat-resistant filler includes aluminum oxide, and the aluminum oxide interacts with the phase change heat storage material to improve the stability and durability of the cable material.

[0008] As an optional implementation, the inorganic high heat-resistant filler includes alumina and silica.

[0009] As an optional embodiment, the content of aluminum oxide is 65-75 wt.%, and the content of silicon dioxide is 25-35 wt.%.

[0010] As an optional embodiment, the phase change heat storage material includes metal hydroxide.

[0011] As an optional embodiment, the metal hydroxide includes at least one of magnesium hydroxide, zinc hydroxide and aluminum hydroxide.

[0012] As an optional implementation, the phase change heat storage material is packaged in a microencapsulated manner.

[0013] As an optional embodiment, the base resin includes 55-65 parts of polyethylene (PE), 20-25 parts of polyvinyl chloride (PVC) and 15-20 parts of polyetheretherketone (PEEK).

[0014] As an optional embodiment, the cross-linking agent includes at least one of dibenzoyl peroxide, dicumyl peroxide and vinyltrimethoxysilane.

[0015] As an optional embodiment, the antioxidant includes at least one of the antioxidant 1010 , the antioxidant 626 and the antioxidant 300 .

[0016] According to a second aspect of the present invention, there is provided a method for preparing the aforementioned high heat-resistant self-cooling energy storage insulating cable material, comprising the following steps:

[0017] Weigh each component by weight, and then place each component in a closed mixer for mixing to obtain a mixture;

[0018] The mixture is added into a twin-screw extruder for melting and mixing, and then extruded and pelletized to obtain the desired cable material.

[0019] It can be seen from the above technical solutions of the present invention that the high heat-resistant self-cooling energy storage insulating cable material proposed by the present invention, on the one hand, adopts a matrix resin composed of polyethylene, polyvinyl chloride and polyetheretherketone as a base material, which ensures the basic performance of insulation and enhances its heat resistance; on the other hand, an alumina and silica composite material is adopted as an inorganic high heat-resistant filler, and the composite material improves the heat resistance of the cable, avoiding breakdown or electrical failure due to high temperature during cable operation;

[0020] Among them, alumina has high thermal conductivity, good insulation performance and chemical stability, which improves the insulation performance of the cable and plays a role in heat dissipation. In high-temperature operation, heat is quickly transferred to the phase change heat storage material through alumina, and the phase change heat storage material reaches the melting point faster, and the material begins to melt and absorb heat, thereby reducing the cable temperature; when the cable temperature drops, the phase change heat storage material solidifies faster under the action of alumina and stores heat. When the cable operates at low temperatures, the heat stored in the phase change heat storage material is quickly released again under the action of alumina, thereby stabilizing the operating temperature of the cable within an appropriate range, greatly increasing the performance and operating temperature range of the system, and can still operate stably at 180°C. Through the interaction between alumina and phase change heat storage materials, the cable has better stability and durability, the cable performance is more stable, and the aging process of the cable material is slowed down, increasing the service life of the cable, thereby ensuring the performance of the system. DETAILED DESCRIPTION

[0021] The embodiments of the present disclosure are not necessarily intended to include all aspects of the invention.It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.

[0022] The present invention adopts polyethylene, polyvinyl chloride and polyetheretherketone to form a matrix resin as an insulating material, adds alumina and silica composite materials as an inorganic high heat-resistant filler, and mixes in phase change heat storage materials to perform cooling and energy storage in the form of energy conversion. The material not only helps the cable material to achieve high temperature resistance and self-cooling performance, avoids hidden dangers such as breakdown and electrical failure, and further ensures the safety of the cable material, but also has an energy storage function, ensures the performance of the cable at low temperatures, and increases the temperature range of the system. In particular, through the interaction between alumina and phase change heat storage materials, the cable has better stability and durability, ensures the stable performance of the cable, and increases the service life of the cable.

[0023] In an exemplary embodiment of the present invention, a high heat-resistant self-cooling energy storage insulating cable material is provided, which comprises the following components by weight: 100 parts of base resin, 20-30 parts of inorganic high heat-resistant filler, 10-15 parts of phase change heat storage material, 5-10 parts of cross-linking agent, 1-3 parts of antioxidant, 2-5 parts of plasticizer, 1-3 parts of stabilizer, and 1-3 parts of stearic acid;

[0024] Among them, the inorganic high heat-resistant filler includes alumina, and the alumina interacts with the phase change heat storage material to improve the stability and durability of the cable material.

[0025] As optional examples, the inorganic high heat-resistant filler includes alumina and silica.

[0026] As an optional example, the content of aluminum oxide is 65 to 75 wt.%, and the content of silicon dioxide is 25 to 35 wt.%.

[0027] As an optional example, the phase change heat storage material includes a metal hydroxide.

[0028] As an optional example, the metal hydroxide includes at least one of magnesium hydroxide, zinc hydroxide, and aluminum hydroxide.

[0029] As an optional example, the phase change heat storage material is packaged in a microencapsulated manner. The microencapsulation form can prevent leakage of the phase change heat storage material, and the phase change heat storage material and alumina can interact better, further improving the stability of the cable.

[0030] In a specific embodiment, the phase change heat storage material can be microencapsulated by spray drying, by mixing the liquid or dissolved phase change heat storage material with the capsule wall material, then spraying it into a mist, and drying it in hot air to form tiny capsules.

[0031] In a typical example, taking the microencapsulation of aluminum hydroxide as an example, the process is as follows:

[0032] Aluminum hydroxide was added to water (0.05 g / mL) and treated with an ultrasonic oscillator for 30 minutes to obtain a uniform suspension; polyvinyl alcohol was added to water (0.1 g / mL) and stirred until completely dissolved to form a solution; the aluminum hydroxide suspension was mixed with the polyvinyl alcohol solution (volume ratio 1:1) to obtain a uniform mixed solution.

[0033] The mixed liquid is loaded into the feed system of the spray dryer, the liquid mixture is sprayed into fine droplets through the nozzle, and quickly dried in hot air, and the dried microcapsule powder is collected.

[0034] Among them, the conditions for spray drying are: inlet air temperature: generally set to 150-200°C, outlet air temperature: generally set to 80-100°C, nozzle pressure: generally set to 0.5-1.5MPa.

[0035] As an optional example, the base resin includes 55-65 parts of polyethylene (PE), 20-25 parts of polyvinyl chloride (PVC), and 15-20 parts of polyetheretherketone (PEEK).

[0036] As an optional example, the cross-linking agent includes at least one of dibenzoyl peroxide, dicumyl peroxide, and vinyltrimethoxysilane.

[0037] As an optional example, the antioxidant includes at least one of the antioxidant 1010 , the antioxidant 626 , and the antioxidant 300 .

[0038] As optional examples, the plasticizer and stabilizer may be selected from commonly used substances in the art, such as the plasticizer tri(2-ethylhexyl) trimellitate (TOTM) and the liquid calcium zinc stabilizer.

[0039] In another exemplary embodiment of the present invention, a method for preparing the aforementioned high heat-resistant self-cooling energy storage insulating cable material is provided, comprising the following steps:

[0040] Weigh each component by weight, and then place each component in a closed mixer for mixing to obtain a mixture;

[0041] The mixture is added into a twin-screw extruder for melting and mixing, and then extruded and pelletized to obtain the desired cable material.

[0042] As an optional example, the components are placed in a closed mixer for mixing, with a high-speed rotation of 350-550 rpm and a mixing time of 10-15 minutes.

[0043] As an optional example, the rotation speed of the twin-screw extruder is 300-500 rpm, and the processing temperature is 220-260°C.

[0044] For better understanding, the present invention is further described below in conjunction with several specific examples, but the preparation process is not limited thereto, and the content of the present invention is not limited thereto.

[0045] Unless otherwise specified, the materials in the examples were prepared according to existing methods or directly purchased from the market.

[0046] The following examples use a spray drying method to microencapsulate the phase change heat storage material. The specific method is as follows:

[0047] Aluminum hydroxide was added to water (0.05 g / mL) and treated with an ultrasonic oscillator for 30 minutes to obtain a uniform suspension; polyvinyl alcohol was added to water (0.1 g / mL) and stirred until completely dissolved to form a solution; the aluminum hydroxide suspension was mixed with the polyvinyl alcohol solution (volume ratio 1:1) to obtain a uniform mixed solution.

[0048] The mixed liquid is loaded into the feed system of the spray dryer, the liquid mixture is sprayed into fine droplets through the nozzle, and quickly dried in hot air, and the dried microcapsule powder is collected.

[0049] The spray drying conditions are as follows: air inlet temperature: 180°C, air outlet temperature: 90°C, and nozzle pressure: 1.0 MPa.

[0050] Example 1

[0051] 55 parts of polyethylene (PE), 25 parts of polyvinyl chloride (PVC), 20 parts of polyetheretherketone (PEEK), 15 parts of aluminum oxide, 15 parts of silicon dioxide, 12 parts of magnesium hydroxide, 5 parts of dibenzoyl peroxide, 1 part of antioxidant (1010), 5 parts of TOTM, 3 parts of liquid calcium zinc stabilizer, and 2 parts of stearic acid.

[0052] Step (1): 100 parts of base resin, 30 parts of inorganic high heat-resistant filler, 12 parts of phase change heat storage material, 5 parts of cross-linking agent, 3 parts of antioxidant, 5 parts of plasticizer, 3 parts of stabilizer, and 2 parts of stearic acid are placed in a closed mixer and mixed at a high speed (speed of 500 rpm) for 12 minutes to obtain a mixture;

[0053] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 450 rpm and the processing temperature is 250°C.

[0054] Example 2

[0055] 63 parts of polyethylene (PE), 18 parts of polyvinyl chloride (PVC), 19 parts of polyetheretherketone (PEEK), 15 parts of aluminum oxide, 15 parts of silicon dioxide, 15 parts of zinc hydroxide, 10 parts of vinyltrimethoxysilane, 3 parts of antioxidant (626), 4 parts of TOTM, 2 parts of liquid calcium zinc stabilizer, and 1 part of stearic acid.

[0056] Step (1): 100 parts of base resin, 25 parts of inorganic high heat-resistant filler, 15 parts of phase change heat storage material, 10 parts of cross-linking agent, 3 parts of antioxidant, 4 parts of plasticizer, 2 parts of stabilizer, and 1 part of stearic acid are placed in a closed mixer for high-speed rotation mixing (rotation speed of 450 rpm) for 15 minutes to obtain a mixture;

[0057] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 400 rpm and the processing temperature is 260°C.

[0058] Example 3

[0059] 60 parts of polyethylene (PE), 23 parts of polyvinyl chloride (PVC), 17 parts of polyetheretherketone (PEEK), 10 parts of aluminum oxide, 10 parts of silicon dioxide, 13 parts of aluminum hydroxide, 5 parts of graphene, 7 parts of dicumyl peroxide, 2 parts of antioxidant (300), 2 parts of TOTM, 1 part of liquid calcium zinc stabilizer, and 3 parts of stearic acid.

[0060] Step (1): 100 parts of base resin, 20 parts of inorganic high heat-resistant filler, 13 parts of phase change heat storage material, 10 parts of energy storage material, 7 parts of cross-linking agent, 2 parts of antioxidant, 2 parts of plasticizer, 1 part of stabilizer, and 3 parts of stearic acid are placed in a closed mixer for high-speed rotation mixing (rotation speed of 530 rpm) for 10 minutes to finally obtain a mixture;

[0061] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 350 pm and the processing temperature is 220°C.

[0062] Comparative Example 1

[0063] Step (1): 100 parts of base resin, 15 parts of inorganic high heat-resistant filler, 2 parts of cross-linking agent, 1 part of antioxidant, 2 parts of TOTM, 1 part of liquid calcium zinc stabilizer, and 2 parts of stearic acid are placed in a closed mixer and mixed at a high speed (rotation speed of 450 pm) for 10 minutes to obtain a mixture;

[0064] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 250 rpm and the processing temperature is 200°C.

[0065] Comparative Example 2

[0066] Step (1): 100 parts of base resin, 18 parts of inorganic high heat-resistant filler, 5 parts of crosslinking agent, 3 parts of antioxidant, 3 parts of TOTM, 3 parts of liquid calcium zinc stabilizer, and 1 part of stearic acid are placed in a closed mixer and mixed at a high speed (rotation speed of 450 pm) for 10 minutes to obtain a mixture;

[0067] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 400 rpm and the processing temperature is 300°C.

[0068] Comparative Example 3

[0069] Step (1): 100 parts of base resin, 10 parts of inorganic high heat-resistant filler, 5 parts of aluminum hydroxide, 3 parts of cross-linking agent, 2 parts of antioxidant, 3 parts of TOTM, 2 parts of liquid calcium zinc stabilizer, and 2 parts of stearic acid are placed in a closed mixer and mixed at a high speed (rotation speed of 400 pm) for 15 minutes to obtain a mixture;

[0070] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 300 rpm and the processing temperature is 250°C.

[0071] Comparative Example 4

[0072] Step (1): 100 parts of base resin, 7 parts of inorganic high heat-resistant filler, 13 parts of aluminum hydroxide, 3 parts of cross-linking agent, 2 parts of antioxidant, 3 parts of TOTM, 1 part of liquid calcium zinc stabilizer, and 2 parts of stearic acid are placed in a closed mixer and mixed at a high speed (rotation speed of 400 pm) for 15 minutes to obtain a mixture;

[0073] Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt mixing, extruding and pelletizing to obtain the desired cable material, wherein the rotation speed of the twin-screw extruder is 300 rpm and the processing temperature is 250°C.

[0074] The formulation compositions of Examples 1 to 3 and Comparative Examples 1 to 4 are shown in Table 1.

[0075] Table 1

[0076]

[0077]

[0078] The performance tests were performed on the sheath layers of the cables prepared in Examples 1 to 3 and Comparative Examples 1 to 4, respectively.

[0079] The test is carried out according to the methods in the test standards such as IEC 60811-1-1-1993 "General test methods for cable insulation and sheath materials" and GB 1040-92 "Test methods for tensile properties of plastics".

[0080] Low temperature resistance: After placing the cable samples in an environment of -45°C for 7 days, the elongation at break is tested in accordance with GB / T 3512-2014 and the elongation at break is calculated.

[0081] The test results of the material samples are listed in Table 2.

[0082] Table 2

[0083]

[0084] By comparing the data of Examples 1 to 3 and Comparative Examples 1 to 4, it is found that compared with Comparative Examples 1 to 4, the tensile strength and elongation at break of the sheath layer of the cable prepared in Examples 1 to 3 at high temperatures are maintained at a higher level, indicating that polyethylene and polyvinyl chloride are used as the matrix materials of the sheath layer of the cable, polyetheretherketone is added, and is combined with a composite material of alumina and polysilicon dioxide. At the same time, under the synergistic effect of alumina and phase change heat storage material, the phase change heat storage material quickly absorbs heat, effectively reduces the temperature of the cable, delays the aging speed of the cable sheath layer at a high temperature of 180°C, has a longer thermal stability time, and improves the toughness of the cable sheath layer, which can significantly improve the high temperature resistance and thermal stability of the cable.

[0085] The elongation at break of the cable was tested under low temperature conditions. It was found that although the phase change heat storage material in Comparative Example 4 can help the cable maintain a certain flexibility to a certain extent, the lack of the support of alumina means that the performance of the cable at extreme low temperatures is not as stable as that of Examples 1 to 3, showing a lower resistance to brittle fracture. In Comparative Example 2, due to the lack of heat release function of the phase change heat storage material at low temperatures, the cable showed weak adaptability in sudden temperature changes. The cables of Examples 1 to 3 release heat quickly at appropriate temperatures through the synergistic effect of alumina and phase change heat storage materials, effectively maintaining the flexibility and mechanical strength of the cable and having good low temperature resistance.

[0086] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A high heat-resistant self-cooling energy storage insulating cable material, characterized in that: The composition comprises the following components by weight: 100 parts of base resin, 20-30 parts of inorganic high heat-resistant filler, 10-15 parts of phase change heat storage material, 5-10 parts of cross-linking agent, 1-3 parts of antioxidant, 2-5 parts of plasticizer, 1-3 parts of stabilizer and 1-3 parts of stearic acid; Among them, the inorganic high heat-resistant filler includes aluminum oxide, and the aluminum oxide interacts with the phase change heat storage material to improve the stability and durability of the cable material.

2. The high heat-resistant self-cooling energy storage insulating cable material according to claim 1, characterized in that: The inorganic high heat-resistant filler includes alumina and silica.

3. The high heat-resistant self-cooling energy storage insulating cable material according to claim 2, characterized in that: The content of aluminum oxide is 65-75 wt.%, and the content of silicon dioxide is 25-35 wt.%.

4. The high heat-resistant self-cooling energy storage insulating cable material according to claim 1, characterized in that: The phase-change heat storage material includes metal hydroxide.

5. The high heat-resistant self-cooling energy storage insulating cable material according to claim 4, characterized in that: The metal hydroxide includes at least one of magnesium hydroxide, zinc hydroxide and aluminum hydroxide.

6. The high heat-resistant self-cooling energy storage insulating cable material according to claim 1, characterized in that: The phase change heat storage material is packaged in a microencapsulated manner.

7. The high heat-resistant self-cooling energy storage insulating cable material according to claim 1, characterized in that: The matrix resin includes 55-65 parts of polyethylene (PE), 20-25 parts of polyvinyl chloride (PVC) and 15-20 parts of polyetheretherketone (PEEK).

8. The high heat-resistant self-cooling energy storage insulating cable material according to claim 1, characterized in that: The crosslinking agent includes at least one of dibenzoyl peroxide, dicumyl peroxide and vinyl trimethoxy silane.

9. The high heat-resistant self-cooling energy storage insulating cable material according to claim 1, characterized in that: The antioxidant includes at least one of the antioxidant 1010 , the antioxidant 626 , and the antioxidant 300 .

10. A method for preparing the high heat-resistant self-cooling energy storage insulating cable material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Weigh each component by weight, and then place each component in a closed mixer for mixing to obtain a mixture; The mixture is added into a twin-screw extruder for melting and mixing, and then extruded and pelletized to obtain the desired cable material.