High-salt-tolerance flame-retardant easy-to-separate metal hose coating long-chain nylon material and preparation method thereof

By using components such as long-chain nylon PA1012 medium adhesive resin and appropriate amount of toughening agent, a high salt-resistant, flame-retardant and easy-to-detach metal hose coating material is prepared, which solves the problem of poor leakage and detachability of metal hose in high-salt environments. Excellent salt resistance and flame retardant properties in high salt environments are achieved.

CN119039873APending Publication Date: 2024-11-29ORINKO HIGH PERFORMANCE MATERIALS TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411107229.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing metal hoses are prone to leakage and poor disengagement in high-salt environments, and lack weathering and aging resistance, making it difficult to meet the safety requirements for beach use.

Method used

Using long-chain nylon PA1012 medium-adhesive resin as the matrix, combined with toughening agent, flame retardant, nucleating agent and other components, a high salt-resistant, flame retardant and easy to detach from the metal hose coating material through the twin-screw extrusion mechanism is used to improve the material flexibility, chemical reagent resistance and detachability.

Benefits of technology

Maintain excellent flexibility and bending performance under -40 degrees, ensure long-term use of the product in high-salt environment, enhance the bonding and disengagement effect between resin and metal hose, and ensure the product's efficient salt resistance and resistance Fueling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991171220000071
    Figure BDA0004991171220000071
  • Figure BDA0004991171220000081
    Figure BDA0004991171220000081
Patent Text Reader

Abstract

The invention discloses a high-salt-tolerance flame-retardant easy-to-separate metal hose coating long-chain nylon material and a preparation method thereof. The high-salt-tolerance flame-retardant easy-to-separate metal hose coating long-chain nylon material is prepared from the following components in percentage by mass: 6-9% of a flexibilizer, 10-20% of a flame retardant, 0.4-0.7% of a lubricant, 0.3-0.8% of an antioxidant, 3-5% of a nucleating agent, 0.5-1.5% of an ultraviolet light absorber, 0.2-0.5% of a heat stabilizer, 1-2% of a coloring agent and the balance of PA1012 adhesive resin. According to the invention, long-chain nylon PA1012 sticky resin is used as basic resin, compared with conventional nylon, the nylon has high and low temperature resistance, PA1012 has excellent flexibility in an environment of-40 DEG C, no whitening and outer layer cracking phenomena are found in 200 tests in a bending experiment at 120 DEG C, and especially, the nylon has excellent flexibility in the environment of-40 DEG C after a flexibilizer is added. When the coated metal pipe is subjected to a bending experiment for 300 times, the outer layer is not cracked.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a highly salt-resistant, flame-retardant and easily detachable metal hose coated with a long-chain nylon material and a preparation method thereof. Background Art

[0002] In order to protect cables and improve safety in life and practice, the conventional practice is to add corrugated tube protection outside the cables. In order to facilitate grounding and further improve safety, metal hoses are used. In order to prevent leakage of metal hoses, there is usually a layer of polymer organic material on the outside of the metal hose for protection, and there are special requirements for polymer materials, such as flame retardancy, weather resistance, aging resistance, cold resistance, easy separation from the metal hose, and good salt resistance in seaside environments. Long-chain nylon not only has the general advantages of nylon, but also has excellent salt resistance. In view of the relatively expensive prices of PA12 and PA11 and the low degree of localization, PA1012 is relatively cheap and has mature mass production in China, so this solution uses domestic PA1012. Summary of the invention

[0003] In view of this, the present invention provides a highly salt-resistant, flame-retardant, and easily detachable metal hose coated long-chain nylon material and a preparation method thereof, which uses a long-chain nylon PA1012 medium-viscosity resin as a base resin. Compared with conventional nylon materials, the material has good high and low temperature resistance and excellent flexibility in a low temperature environment. After adding an appropriate amount of toughening agent, nucleating agent, etc. to the system, the material has a good easy-to-form effect.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] In the first aspect, the present invention discloses a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material, which is prepared from the following components by mass percentage:

[0006] Toughener 6-9%, flame retardant 10-20%, lubricant 0.4-0.7%, antioxidant 0.3-0.8%, nucleating agent 3-5%, UV absorber 0.5-1.5%, heat stabilizer 0.2-0.5%, colorant 1-2%, and the remainder of viscous resin in PA1012.

[0007] Further solution: The toughening agent is at least one of grafted POE, grafted EPDM and grafted SEBS, and the fluidity of the toughening agent is lower than 1g / 10min. Too high fluidity of the toughening agent will lead to problems such as difficulty in extrusion and uneven wall thickness.

[0008] A further solution: the flame retardant is at least one of melamine polyphosphate, diethyl aluminum hypophosphite, brominated polystyrene and antimony trioxide.

[0009] A further solution: the lubricant is at least one of PETS, OP wax, silicone, silicone oil and silicone amide.

[0010] A further solution: the antioxidant includes a primary antioxidant and a secondary antioxidant, the primary antioxidant is at least one of antioxidant 245, antioxidant 1010, antioxidant 1098, and antioxidant 9228, and the secondary antioxidant is at least one of antioxidant 168 and antioxidant 626.

[0011] A further solution: the nucleating agent is at least one of CAV102 nucleating agent, P22 nucleating agent and Finner-122 nucleating agent.

[0012] A further solution: the ultraviolet absorber is at least one of UV326 ultraviolet absorber, L20 ultraviolet absorber, UV944 ultraviolet absorber and UV770 ultraviolet absorber.

[0013] A further solution: the heat stabilizer is at least one of an inorganic copper salt nylon heat stabilizer, an organic copper salt nylon heat stabilizer, an inorganic phosphate nylon heat stabilizer, an aluminum silicate treated with titanate, and a dipentaerythritol (3-(3.5-tert-butyl-4-hydroxyphenyl) propionate) composite heat stabilizer.

[0014] Further solution: The relative viscosity of the adhesive resin in PA1012 is 5.

[0015] In a second aspect, the present invention discloses a method for preparing the above-mentioned highly salt-resistant, flame-retardant and easily detachable metal hose coated with a long-chain nylon material, comprising the following steps:

[0016] Weigh each component according to mass percentage, mix the binder resin, toughening agent and colorant in PA1012 evenly, then add flame retardant, lubricant, nucleating agent, antioxidant, ultraviolet absorber and heat stabilizer and mix evenly to obtain a mixture;

[0017] The mixed material is added into the main feeding port of the twin-screw extruder, and after melting, extrusion, cooling, air drying and pelletizing, a highly salt-resistant, flame-retardant and easily detachable metal hose coated with a long-chain nylon material is obtained;

[0018] Among them, the temperature of the twin-screw extruder from the first zone to the head is 215°C, 225°C, 235°C, 235°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C; the screw speed is 300 rpm and the feeding is 25-30 rpm.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention uses long-chain nylon PA1012 medium-viscosity resin as the base resin. Compared with conventional nylon, PA1012 has high and low temperature resistance. PA1012 also has excellent flexibility in an environment of -40 degrees. No whitening or outer layer cracking was found in the 120-degree bending test for 200 times. In particular, after adding a toughening agent, the coated metal tube was subjected to a bending test for 300 times in an environment of -40 degrees, and no outer layer cracking was found;

[0021] 2. The present invention uses long-chain nylon PA1012 medium-viscosity resin as the base resin. Compared with conventional nylon, it not only has excellent chemical resistance, but also has very good salt resistance, ensuring that the product can be used for a long time in an environment with high salt content;

[0022] 3. The present invention uses long-chain nylon PA1012 medium-viscosity resin as the base resin and adds some toughening agent. Our test found that too low addition of toughening agent grafted POE will result in low temperature resistance not meeting the standard. When the addition ratio exceeds 10%, the polarity is increased during extrusion molding with the metal hose, which intensifies the bonding between the resin and the metal hose;

[0023] 4. The present invention uses a nucleating agent to improve the rapid crystallization of the resin to achieve the purpose of separating the resin from the metal hose. When the amount of the nucleating agent is less than 2%, the separation rate is less than 99.5%. When the amount of the nucleating agent reaches more than 3%, the separation effect of the resin and the metal hose is very good. At the same time, due to the selection of a specific nucleating agent, such as the P22 nucleating agent, which itself has a nylon monomer part, the compatibility problem is solved. DETAILED DESCRIPTION

[0024] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0026] The specific information of the raw materials used in the following examples and comparative examples is as follows:

[0027] The lubricant is silicone masterbatch, manufactured by Dow Corning, brand MB50-008;

[0028] The main antioxidant is antioxidant 1098, the manufacturer is Tianjin Li'anlong, the brand is RIANOX 1098;

[0029] The secondary antioxidant is antioxidant 168, produced by Tianjin Li'anlong, brand name RIANOX 168;

[0030] Heat stabilizer, manufactured by Brüggemann, brand name H318;

[0031] Colorant, manufactured by Cabot, brand number 2718;

[0032] PA1012 medium viscosity resin, produced by Shandong Dongchen, brand PA1012 medium viscosity, relative viscosity 5;

[0033] Toughening agent, manufactured by Shenyang Ketong, brand KT-915;

[0034] Flame retardant, manufactured by Jiangsu Liside, brand name LFR-8003;

[0035] Nucleating agent, manufactured by Brüggemann, brand name P22;

[0036] Ultraviolet absorber, the manufacturer is Tianjin Lianlong, the brand name is UV944.

[0037] All materials are commercially available common products.

[0038] It is to be understood that the above raw materials and reagents are only examples of some specific embodiments of the present invention, so that the technical solution of the present invention is clearer, and it does not mean that the present invention can only use the above reagents, and the specific scope in the claims shall prevail. In addition, the "parts" described in the examples and comparative examples, unless otherwise specified, refer to parts by weight.

[0039] Any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0040] Example 1

[0041] (1) Weigh the following components in parts by weight: 74 parts of PA1012 neutralizing resin, 6 parts of toughening agent (KT-915), 14 parts of flame retardant, 3 parts of nucleating agent, 1 part of ultraviolet absorber, 0.5 parts of lubricant, 0.3 parts of primary antioxidant, 0.2 parts of secondary antioxidant, 0.3 parts of heat stabilizer, and 1.5 parts of colorant, wherein the PA1012 neutralizing resin is pre-dried at 80°C for 4 hours (Examples 2-3 and Comparative Examples 1-3 are also dried).

[0042] (2) Mixing: Add PA1012 medium viscosity resin, toughening agent, colorant into a high-speed mixer and mix at high speed for 5 minutes, then add flame retardant, lubricant, UV absorber, nucleating agent, antioxidant and heat stabilizer and continue mixing at high speed for 5 minutes to obtain a mixture;

[0043] (3) Melt extrusion: the mixed material is added into the main feed port of a twin-screw extruder, and the temperature of the twin-screw extruder is 215° C., 225° C., 235° C., 235° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C. from the first zone to the die head; the screw speed is 300 rpm, and the feeding speed is 25-30 rpm;

[0044] (4) Extrusion pelletizing: The extruded material is cooled, air-dried, pelletized, passed through a vibrating screen, homogenized in a homogenizing tank, and packaged to obtain a finished product, that is, a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material.

[0045] Example 2

[0046] (1) Weigh the following components in parts by weight: 72 parts of PA1012 neutral binder resin, 8 parts of toughening agent (KT-915), 14 parts of flame retardant, 3 parts of nucleating agent, 1 part of ultraviolet absorber, 0.5 parts of lubricant, 0.3 parts of primary antioxidant, 0.2 parts of secondary antioxidant, 0.3 parts of heat stabilizer, and 1.5 parts of colorant.

[0047] (2) Mixing: Add PA1012 medium viscosity resin, toughening agent, colorant into a high-speed mixer and mix at high speed for 5 minutes, then add flame retardant, lubricant, UV absorber, nucleating agent, antioxidant and heat stabilizer and continue mixing at high speed for 5 minutes to obtain a mixture;

[0048] (3) Melt extrusion: the mixed material is added into the main feed port of a twin-screw extruder, and the temperature of the twin-screw extruder is 215° C., 225° C., 235° C., 235° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C. from the first zone to the die head; the screw speed is 300 rpm, and the feeding speed is 25-30 rpm;

[0049] (4) Extrusion pelletizing: The extruded material is cooled, air-dried, pelletized, passed through a vibrating screen, homogenized in a homogenizing tank, and packaged to obtain a finished product, that is, a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material.

[0050] Example 3

[0051] (1) Weigh the following components in parts by weight: 70.0 parts of PA1012 neutral binder resin, 9 parts of toughening agent (KT-915), 14 parts of flame retardant, 4 parts of nucleating agent, 1 part of ultraviolet absorber, 0.5 parts of lubricant, 0.3 parts of primary antioxidant, 0.2 parts of secondary antioxidant, 0.3 parts of heat stabilizer, and 1.5 parts of colorant.

[0052] (2) Mixing: Add weighed PA1012 medium-viscosity resin, toughening agent, and colorant into a high-speed mixer and mix at high speed for 5 minutes, then add weighed flame retardant, lubricant, UV absorber, nucleating agent, antioxidant, and heat stabilizer and continue mixing at high speed for 5 minutes to obtain a mixture;

[0053] (3) Melt extrusion: the mixed material is added into the main feed port of a twin-screw extruder, and the temperature of the twin-screw extruder is 215° C., 225° C., 235° C., 235° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C. from the first zone to the die head; the screw speed is 300 rpm, and the feeding speed is 25-30 rpm;

[0054] (4) Extrusion pelletizing: The extruded material is cooled, air-dried, pelletized, passed through a vibrating screen, homogenized in a homogenizing tank, and packaged to obtain a finished product, that is, a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material.

[0055] Comparative Example 1

[0056] (1) Weigh the following components in parts by weight: 72 parts of PA1012 binder resin, 10 parts of toughening agent (KT-915), 14 parts of flame retardant, 3 parts of nucleating agent, 1 part of ultraviolet absorber, 0.5 parts of lubricant, 0.3 parts of primary antioxidant, 0.2 parts of secondary antioxidant, 0.3 parts of heat stabilizer, and 1.5 parts of colorant.

[0057] (2) Mixing: Add PA1012 medium viscosity resin, toughening agent, and colorant into a high-speed mixer and mix at high speed for 5 minutes, then add weighed flame retardant, lubricant, UV absorber, nucleating agent, antioxidant, and heat stabilizer and continue mixing at high speed for 5 minutes to obtain a mixture;

[0058] (3) Melt extrusion: the mixed material is added into the main feed port of a twin-screw extruder, and the temperature of the twin-screw extruder is 215° C., 225° C., 235° C., 235° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C. from the first zone to the die head; the screw speed is 300 rpm, and the feeding speed is 25-30 rpm;

[0059] (4) Extrusion pelletizing: The extruded material is cooled, air-dried, pelletized, passed through a vibrating screen, homogenized in a homogenizing tank, and packaged to obtain a finished product, that is, a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material.

[0060] Comparative Example 2

[0061] (1) Weigh the following components in parts by weight: 72 parts of PA1012 binder resin, 8 parts of toughening agent (KT-915), 14 parts of flame retardant, 2 parts of nucleating agent, 1 part of ultraviolet absorber, 0.5 parts of lubricant, 0.3 parts of primary antioxidant, 0.2 parts of secondary antioxidant, 0.3 parts of heat stabilizer, and 1.5 parts of colorant.

[0062] (2) Mixing: Add PA1012 medium viscosity resin, toughening agent, colorant into a high-speed mixer and mix at high speed for 5 minutes, then add flame retardant, lubricant, ultraviolet absorber, nucleating agent, primary and auxiliary antioxidants and thermal stabilizer and continue to mix at high speed for 5 minutes to obtain a mixture;

[0063] (3) Melt extrusion: the mixed material is added into the main feed port of a twin-screw extruder, and the temperature of the twin-screw extruder is 215° C., 225° C., 235° C., 235° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C., 240° C. from the first zone to the die head; the screw speed is 300 rpm, and the feeding speed is 25-30 rpm;

[0064] (4) Extrusion pelletizing: The extruded material is cooled, air-dried, pelletized, passed through a vibrating screen, homogenized in a homogenizing tank, and packaged to obtain a finished product, that is, a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material.

[0065] Comparative Example 3

[0066] (1) Weigh the following components in parts by weight: 70 parts of PA1012 binder resin, 8 parts of toughening agent (KT-915), 14 parts of flame retardant, 5 parts of nucleating agent, 1 part of ultraviolet absorber, 0.5 parts of lubricant, 0.3 parts of primary antioxidant, 0.2 parts of secondary antioxidant, 0.3 parts of heat stabilizer, and 1.5 parts of colorant.

[0067] (2) Mixing: Add PA1012 medium viscosity resin, toughening agent, colorant into a high-speed mixer and mix at high speed for 5 minutes, then add flame retardant, lubricant, UV absorber, nucleating agent, antioxidant and heat stabilizer and continue mixing at high speed for 5 minutes to obtain a mixture;

[0068] (3) Melt extrusion: The mixed material is added into the main feed port of a twin-screw extruder. The temperature of the twin-screw extruder is 215°C, 225°C, 235°C, 235°C, 240°C, 240°C, 240°C, 240°C, 215°C, 225°C, 235°C, 240 ...

[0069] 240℃, 240℃, 240℃, 240℃; screw speed is 300 rpm, feeding is 25-30 rpm;

[0070] (4) Extrusion pelletizing: The extruded material is cooled, air-dried, pelletized, passed through a vibrating screen, homogenized in a homogenizing tank, and packaged to obtain a finished product, that is, a highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material.

[0071] Test Case

[0072] Performance tests were performed on Examples 1-3, Comparative Examples 1-3, and the highly salt-resistant, flame-retardant, and easily detachable metal hose coated long-chain nylon material prepared in the Comparative Examples. The performance test methods, conditions, and test results are shown in Table 1.

[0073] Table 1

[0074]

[0075]

[0076] The detachment experiment was performed as follows:

[0077] Take the formed coated metal hose, select three discontinuous sections of the hose, cut it along the length of the hose with a knife, measure the ratio of the completely detached length to the 1-meter length in units of 1 meter, and take the average value.

[0078] The bending test is carried out in the following manner:

[0079] Cut three sections of coated metal hose with a length of 500±20 mm, place them in an environment of -40 degrees for 12 hours and then bend them. The bending angle is not less than 120 degrees, the bending frequency is 5-25 times / minute, and they are bent 200 times. If there are no obvious creases or cracks on the outer plastic coating of the metal hose, it is qualified. If there are obvious creases and cracks in one section, it can be judged that the bending test has failed.

[0080] From the above data analysis, it can be seen that the nylon materials prepared in Examples 1-3 have good separation performance between the resin and the metal hose during the molding process, and have good low-temperature bending performance and impact performance.

[0081] In Comparative Example 1, the amount of toughening agent exceeds 10%. Even if the amount of nucleating agent is increased, the adhesion brought by the increase in material polarity exceeds the detachment effect of the nucleating agent, the detachment rate does not meet the standard, and the flame retardant performance is compromised.

[0082] In Comparative Example 2, the amount of nucleating agent used was less than 2%, and the detachment rate of the resin and the metal hose did not meet the standard.

[0083] In Comparative Example 3, the amount of nucleating agent used was higher than 6%, and the detachment rate of the resin and the metal hose met the standard, but the low-temperature bending performance was poor.

[0084] Although this specification is described according to implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0085] Therefore, the above description is only a preferred embodiment of the present application and is not intended to limit the scope of implementation of the present application; that is, all equivalent changes made according to the scope of the claims of the present application are within the protection scope of the claims of the present application.

Claims

1. A highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material, characterized in that: It is prepared by the following components in percentage by mass: Toughener 6-9%, flame retardant 10-20%, lubricant 0.4-0.7%, antioxidant 0.3-0.8%, nucleating agent 3-5%, UV absorber 0.5-1.5%, heat stabilizer 0.2-0.5%, colorant 1-2%, and the remainder of viscous resin in PA1012.

2. The highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material according to claim 1, characterized in that: The toughening agent is at least one of grafted POE, grafted EPDM and grafted SEBS, and the fluidity of the toughening agent is lower than 1g / 10min.

3. The highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material according to claim 1, characterized in that: The flame retardant is at least one of melamine polyphosphate, diethyl aluminum hypophosphite, brominated polystyrene and antimony trioxide.

4. The highly salt-resistant, flame-retardant and easily detachable metal hose coated with long-chain nylon material according to claim 1, characterized in that: The lubricant is at least one of PETS, OP wax, silicone, silicone oil and silicone amide.

5. The highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material according to claim 1, characterized in that: The antioxidant includes a primary antioxidant and a secondary antioxidant. The primary antioxidant is one of antioxidant 245, antioxidant 1010, antioxidant 1098, and antioxidant 9228; the secondary antioxidant is one of antioxidant 168 and antioxidant 626.

6. The highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material according to claim 1, characterized in that: The nucleating agent is at least one of CAV102 nucleating agent, P22 nucleating agent and Finner-122 nucleating agent.

7. The highly salt-resistant, flame-retardant, and easily detachable metal hose coated with a long-chain nylon material according to claim 1, characterized in that: The ultraviolet absorber is at least one of UV326 ultraviolet absorber, L20 ultraviolet absorber, UV944 ultraviolet absorber and UV770 ultraviolet absorber.

8. The highly salt-resistant, flame-retardant and easily detachable metal hose coated with long-chain nylon material according to claim 1, characterized in that: The heat stabilizer is at least one of an inorganic copper salt nylon heat stabilizer, an organic copper salt nylon heat stabilizer, an inorganic phosphate nylon heat stabilizer, an aluminum silicate treated with titanate, and a dipentaerythritol (3-(3.5-tert-butyl-4-hydroxyphenyl) propionate) composite heat stabilizer.

9. The highly salt-resistant, flame-retardant and easily detachable metal hose coated with long-chain nylon material according to claim 1, characterized in that: The relative viscosity of the adhesive resin in PA1012 is 5.

10. The method for preparing the highly salt-resistant, flame-retardant and easily detachable metal hose coated with long-chain nylon material as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: Weigh each component according to mass percentage, mix the binder resin, toughening agent and colorant in PA1012 evenly, then add flame retardant, lubricant, nucleating agent, antioxidant, ultraviolet absorber and heat stabilizer and mix evenly to obtain a mixture; The mixed material is added into the main feeding port of the twin-screw extruder, and after melting, extrusion, cooling, air drying and pelletizing, a highly salt-resistant, flame-retardant and easily detachable metal hose coated with a long-chain nylon material is obtained; Among them, the temperature of the twin-screw extruder from the first zone to the head is 215°C, 225°C, 235°C, 235°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C, 240°C; the screw speed is 300 rpm and the feeding is 25-30 rpm.

Citation Information

Patent Citations

  • Antistatic anti-flaming polyamide compound and preparation method thereof

    CN106519662A

  • Preparation method of polyamide material for pipe coating

    CN110117415A

  • Wear-resistant reinforced long-carbon-chain nylon PA1012 composite material and preparation method thereof