Organic micro-nano eutectic material, preparation method and application
By growing organic micro-nano eutectic materials in situ in thermoplastic polyurethane fibers, the problem of difficulty in achieving continuous macro-preparation in the prior art is solved, and the preparation of organic micro-nano eutectic materials with regular morphology and adjustable emission wavelength is realized. , expanding its application in the field of OLED.
Patent Information
- Application Number
- CN202411015766.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to realize the continuous macro preparation of organic micro-nano eutectic materials with regular morphology, which limits its wide application in the OLED field.
Using chemical spinning strategy, organic micro-nano eutectic materials are grown in situ in solidification bath by doping organic donor and acceptor materials in thermoplastic polyurethane fibers, and rod-shaped by sonication and centrifugal drying. Organic micro-nano eutectics.
The continuous preparation of organic micro-nano eutectic materials with regular morphology, adjustable emission wavelength, high luminous intensity, uniformity and stable performance has been achieved, and its application in the fields of fluorescence display, lighting, anti-counterfeiting and sensing has been expanded.
Smart Images

Figure CN119039971A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material preparation and application, and relates to an organic micro-nano eutectic, a continuous preparation method and application. Background Art
[0002] Organic semiconductors are widely used in the field of OLEDs due to their excellent luminescence performance and high biocompatibility (see reference: Chem Rev. 2023, 123, 8232-8250), but there are problems with chemical modification and complex synthesis; organic micro-nano eutectic materials are synthesized through eutectic engineering strategies, which can avoid the complex modification process of a single organic semiconductor. Therefore, they have become a hot topic in organic semiconductor research and are expected to be used as a new type of semiconductor material in the field of OLEDs (see reference: AngewChem Int Edit. 2017, 56: 7831-7835). As a new type of organic semiconductor, organic micro-nano eutectic materials have the characteristics of easy control of morphology and fluorescence emission and simple synthesis. However, organic micro-nano eutectic materials with regular morphology can only be synthesized in milligrams at present, and it is difficult to achieve continuous large-scale preparation (see reference: CCS Chemistry. 2021, 3,413-424). Summary of the invention
[0003] In view of the deficiency in the prior art that it is difficult to realize continuous large-scale preparation of organic micro-nano eutectic materials with regular morphology, the present invention provides an organic micro-nano eutectic material with regular morphology, adjustable emission wavelength, high luminous intensity, uniform luminescence and stable performance, a continuous preparation method and application.
[0004] The technical solution to achieve the purpose of the present invention is a method for preparing an organic micro-nano eutectic material, comprising the following steps: (1) Press N,N- A mixed solvent is prepared by mixing dimethylformamide and acetonitrile in a volume ratio of 1:1 to 5:3, and an organic donor and an acceptor material are added, wherein the mass ratio of the organic donor to the acceptor is 1:1 to 1:3, wherein the organic donor is one of naphthalene (NA), triphenylene (BCP), carbazole (Cz) and benzoperylene (BGP), and the acceptor is 1,2,4,5 -tetracyanobenzene (TCNB); then adding 15 to 25 wt% of thermoplastic polyurethane (TPU) by solution mass, treating at room temperature and magnetic stirring conditions until the polyurethane is completely dissolved to obtain a spinning solution; (2) Using deionized water as a coagulation bath, at a temperature of 20 to 25° C. and a humidity of 30 to 45%, the spinning solution prepared in step (1) is spun by a wet spinning process to in-situ grow organic micro-nano eutectics inside and on the surface of the polyurethane fiber to obtain an organic micro-nano eutectic material.
[0005] The method for preparing the organic micro-nano eutectic material of the present invention comprises immersing the organic micro-nano eutectic material in deionized water, and using ultrasonic treatment to peel off the organic micro-nano eutectic material grown on the fiber; then centrifuging to remove the supernatant, and drying the precipitate to obtain a rod-shaped organic micro-nano eutectic material.
[0006] The technical solution of the present invention includes an organic micro-nano eutectic material obtained according to the above preparation method.
[0007] The organic micro-nano eutectic material of the present invention is in the shape of a rod with a length of 5 to 20 µm. Under ultraviolet light excitation, the fluorescence emitted by the organic micro-nano eutectic material is one of sky blue, green, orange and red.
[0008] The present invention provides an application of an organic micro-nano eutectic material, which is used in the fields of fluorescence display, lighting, fluorescence anti-counterfeiting and fluorescence sensing.
[0009] The present invention adopts a chemical spinning strategy to achieve the in-situ growth and continuous preparation of organic micro-nano eutectic materials. The invention principle is: organic donor materials and acceptor materials are doped into TPU fibers, and a wet spinning technology scheme is adopted. When the TPU base material contacts the water in the coagulation bath, it is cross-linked to form fibers. At the same time, the donor and acceptor raw materials are driven by the charge transfer force to grow into organic micro-nano eutectic materials in situ on the surface and inside of the fibers. As the fibers are continuously formed and collected by the fiber collector, the organic micro-nano eutectic materials are also continuously prepared and produced.
[0010] Compared with modern technology, the beneficial effects of the present invention are: by using organic donor materials and acceptor materials, through a wet spinning process, organic micro-nano eutectic materials are prepared in situ inside and on the surface of TPU fibers, providing a continuous large-scale preparation method for organic micro-nano eutectic materials with regular morphology, and expanding the application of organic micro-nano eutectic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 In the figure, (a) and (b) are respectively the SEM image and HR-TEM diffraction image of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 1 of the present invention.
[0012] Figure 2 This is the XRD pattern of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 1 of the present invention.
[0013] Figure 3 In the figure, (a) and (b) are respectively the fluorescence emission spectrum and CIE chromaticity coordinate diagram of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 1 of the present invention.
[0014] Figure 4 In the figure, (a) and (b) are fluorescence microscope images and digital camera images of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 1 of the present invention under ultraviolet light irradiation.
[0015] Figure 5 This is a SEM image of the Cz-TCNB organic micro-nano eutectic material prepared in Example 1 of the present invention after being separated from the fibers.
[0016] Figure 6 This is a fluorescence display effect diagram of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 1 of the present invention.
[0017] Figure 7 This is a fluorescence microscope image of the NA-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 2 of the present invention under ultraviolet light irradiation.
[0018] Figure 8 This is a fluorescence microscope image of the BCP-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 3 of the present invention under ultraviolet light irradiation.
[0019] Fig. 9 This is a fluorescence microscope image of the BGP-TCNB organic micro-nano eutectic material loaded on the fiber prepared in Example 4 of the present invention under ultraviolet light irradiation. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments. Example 1
[0021] 0.1 g carbazole, 0.107 g 1,2,4,5 -Tetracyanobenzene was added to 8 mL N,N 1.2 g of polyurethane (TPU) was added to a mixed solvent of dimethylformamide and acetonitrile (volume ratio of 5:3), and stirred at room temperature for 5 h using a magnetic stirrer until TPU was completely dissolved to obtain a spinning solution.
[0022] The spinning solution was sucked into a 5 mL syringe and fixed on a propulsion pump for wet spinning. An 18G spinning nozzle was used, and the propulsion speed of the syringe was set to 6 mL / h. Spinning was performed at a temperature of 25°C and a humidity of 45%. In a deionized water coagulation bath, a Cz-TCNB organic Wiener eutectic material loaded in TPU fibers was obtained.
[0023] The obtained Cz-TCNB organic Wiener eutectic material was further subjected to ultrasonic exfoliation to obtain pure Cz-TCNB organic micro-nano eutectic material. 300 mL of deionized water was added to a beaker, and 10 g of fiber loaded with Cz-TCNB organic micro-nano eutectic material was completely immersed in it. The Cz-TCNB organic micro-nano eutectic grown on the fiber was exfoliated under ultrasonic conditions of 25°C and 25 kHz; after ultrasonic treatment for 1 h, the supernatant was removed and the precipitate was dried at 7000 r / min to obtain pure Cz-TCNB organic micro-nano eutectic material.
[0024] See attached Figure 1 , (a) is the SEM image of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in this embodiment. It can be seen that 5-20 μm Cz-TCNB organic Wiener eutectic was successfully prepared by wet spinning, and it was located on the surface and inside of the fiber; (b) is the HR-TEM diffraction image of the Cz-TCNB organic micro-nano eutectic loaded on the fiber prepared in this embodiment. It can be seen that the organic micro-nano eutectic material prepared by wet spinning has obvious diffraction points, indicating that it has high crystallinity.
[0025] See attached Figure 2 , is the XRD pattern of the Cz-TCNB organic micro-nano eutectic loaded on the fiber prepared in this embodiment, which has obvious diffraction peaks in the (001), (011), (01-1), and (210) directions, further illustrating that the Cz-TCNB organic Wiener eutectic has extremely strong crystallinity.
[0026] See attached Figure 3 , (a) is the fluorescence emission spectrum of the Cz-TCNB organic micro-nano eutectic loaded on the fiber prepared in this example, and its maximum emission peak is located at 596 nm, which belongs to orange light emission, and the fluorescence quantum yield is 10.6%. (b) is the chromaticity coordinate CIE diagram of the Cz-TCNB organic micro-nano eutectic loaded on the fiber prepared in this example, and its coordinates are (0.527, 0.459), which proves again that it belongs to orange light emission.
[0027] See attached Figure 4 , (a) is a fluorescence microscope image of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in this embodiment under ultraviolet light irradiation. It can be seen that its morphology is rod-shaped and emits uniform orange light under ultraviolet light irradiation; (b) is a digital camera image of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared in this embodiment under ultraviolet light irradiation. It emits uniform orange light under ultraviolet light irradiation and has flexible and bendable characteristics.
[0028] See attached Figure 5, is the SEM image of the Cz-TCNB organic micro-nano eutectic material peeled off from the fiber prepared in this example, Figure 6 It can be seen that the Cz-TCNB organic micro-nano eutectic material is a rod-like structure of 5 to 20 μm, proving that the organic micro-nano eutectic material can be peeled off from the fiber without destroying the structure.
[0029] According to the technical solution provided in this embodiment, the continuous preparation of organic micro-nano eutectic materials can be achieved. A certain amount of fibrous Cz-TCNB organic micro-nano eutectic material is used to prepare a fiber bracelet by a crochet process.
[0030] See attached Figure 6 , which is a fluorescence display effect diagram of the Cz-TCNB organic micro-nano eutectic material loaded on the fiber prepared by the method of this embodiment. It can be seen that the fiber bracelet prepared by crocheting emits orange fluorescence, proving that the Cz-TCNB organic micro-nano eutectic material loaded on the fiber can be used for fluorescence display. Example 2
[0031] 0.2 g naphthalene, 0.214 g 1,2,4,5 -Tetracyanobenzene was added to a mixed solvent of 16 mL of N,N-dimethylformamide and acetonitrile (volume ratio of 5:3), and then 3.0 g of polyurethane (TPU) was added, and stirred at room temperature for 5 h using a magnetic stirrer until TPU was completely dissolved to obtain a spinning solution.
[0032] The spinning solution was sucked into a 5 mL syringe and fixed on a propulsion pump for wet spinning. An 18G spinning nozzle was used, and the propulsion speed of the syringe was set to 6 mL / h. Spinning was performed at a temperature of 25°C and a humidity of 40%. NA-TCNB organic Wiener eutectic material loaded in TPU fiber was obtained in a deionized water coagulation bath.
[0033] See attached Figure 7 , is a fluorescence microscope image of the NA-TCNB organic micro-nano eutectic material loaded on the fiber prepared in this embodiment under ultraviolet light irradiation. It can be seen that the morphology of the organic micro-nano eutectic is rod-shaped with a length of 5 to 20 μm, and emits uniform sky blue light under ultraviolet light irradiation. Example 3
[0034] 0.3 benzophenanthrene, 0.321 g 1,2,4,5 -Tetracyanobenzene was added to 24 mL N,N 4.8 g of polyurethane (TPU) was added to a mixed solvent of dimethylformamide and acetonitrile (volume ratio of 5:3), and stirred at room temperature for 5 h using a magnetic stirrer until TPU was completely dissolved to obtain a spinning solution.
[0035] The spinning solution was sucked into a 5 mL syringe and fixed on a propulsion pump for wet spinning. An 18G spinning nozzle was used, and the propulsion speed of the syringe was set to 8 mL / h. Spinning was performed at a temperature of 20°C and a humidity of 45%. The BCP-TCNB organic Wiener eutectic material loaded in the TPU fiber was obtained in the coagulation bath.
[0036] See attached Figure 8 , is a fluorescence microscope image of the BCP-TCNB organic micro-nano eutectic material loaded on the fiber prepared in this embodiment under ultraviolet light irradiation. It can be seen that the morphology of the organic micro-nano eutectic is rod-shaped with a length of 5 to 20 μm, and emits uniform green light under ultraviolet light irradiation. Example 4
[0037] 0.4 g benzoperylene, 0.856 g 1,2,4,5- Add 32 mL of tetracyanobenzene N,N 6.4 g of polyurethane (TPU) was added to a mixed solvent of dimethylformamide and acetonitrile (volume ratio of 5:3), and stirred at room temperature for 5 h using a magnetic stirrer until TPU was completely dissolved to obtain a spinning solution.
[0038] The spinning solution was sucked into a 5 mL syringe and fixed on a propulsion pump for wet spinning. An 18G spinning nozzle was used, and the propulsion speed of the syringe was set to 6 mL / h. Spinning was performed at a temperature of 25°C and a humidity of 45%. In a coagulation bath of deionized water, a BGP-TCNB organic Wiener eutectic material loaded with BGP-TCNB in TPU fibers was obtained.
[0039] See attached Fig. 9 , which is a fluorescence microscope image of the BGP-TCNB organic micro-nano eutectic material loaded on the fiber prepared in this example under ultraviolet light irradiation. It can be seen that the morphology of the BGP-TCNB organic micro-nano eutectic is a rod-like shape with a length of 5 to 15 μm, and emits uniform red light under ultraviolet light irradiation.
Claims
1. A method for preparing an organic micro-nano eutectic material, characterized in that The following steps are involved: (1) Press N,N- The volume ratio of dimethylformamide to acetonitrile is 1:1 to 5:3 to prepare a mixed solvent, and an organic donor and an acceptor material are added, and the mass ratio of the organic donor to the acceptor is 1:1 to 1:3, the organic donor is one of naphthalene, triphenylene, carbazole and benzoperylene, and the acceptor is 1,2,4,5 -tetracyanobenzene; then adding 15 to 25 wt% of thermoplastic polyurethane by mass of the solution, treating at room temperature and magnetic stirring conditions until the polyurethane is completely dissolved to obtain a spinning solution; (2) Using deionized water as a coagulation bath, at a temperature of 20 to 25° C. and a humidity of 30 to 45%, the spinning solution prepared in step (1) is spun by a wet spinning process to in-situ grow organic micro-nano eutectics inside and on the surface of the polyurethane fiber to obtain an organic micro-nano eutectic material.
2. The method for preparing an organic micro-nano eutectic material according to claim 1, characterized in that: The organic micro-nano eutectic material is immersed in deionized water, and ultrasonic treatment is used to peel off the organic micro-nano eutectic material grown on the fiber; then centrifugation is performed to remove the supernatant, and the precipitate is dried to obtain a rod-shaped organic micro-nano eutectic material.
3. An organic micro-nano eutectic material obtained by the preparation method according to claim 1.
4. The organic micro-nano eutectic material according to claim 3, characterized in that: Organic micro-nano eutectics are rod-shaped with a length of 5 to 20 µm.
5. The organic micro-nano eutectic material according to claim 3, characterized in that: Under ultraviolet light excitation, the fluorescence emitted by the organic micro-nano eutectic material is one of sky blue, green, orange and red.
6. The use of an organic micro-nano eutectic material according to claim 3, characterized in that :Used in the fields of fluorescent display, lighting, fluorescent anti-counterfeiting and fluorescent sensing.
Citation Information
Cited By
Organic charge transfer compound, crystal, preparation method and application
CN119685007A