Monocrystalline silicon texturing additive with strong stain cleaning capability and texturing method
By using macromolecular sugars, suede regulators, cleaning additives and anionic surfactants in the velvet making process of single crystal silicon cell, a one-step velvet making strong stain cleaning is achieved, and surface pollution is solved and residual problems improve battery performance and production efficiency and reduce chemical consumption.
Patent Information
- Application Number
- CN202411129434.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, during the shredding process of single crystal silicon cell, it is difficult to completely remove surface contamination and residues, which affects the preparation of P-N junctions and battery performance, and the cleaning chemicals consume a lot, increasing production costs.
Using a velvet-making additive including macromolecular sugars, suede regulators, cleaning additives and anionic surfactants, a strong stain cleaning is achieved through one-step velvet making, forming a uniform microstructure and a high specific surface area suede to reduce Chemical usage.
Effectively remove pollution and residues on the surface of single crystal silicon wafers, improve battery efficiency and yield, reduce chemical consumption, reduce production costs, and improve process stability and production line efficiency.
Smart Images

Figure CN119039990A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a monocrystalline silicon texturing additive and a texturing method with strong contamination cleaning ability, belonging to the technical field of photovoltaic monocrystalline silicon cell manufacturing. Background Art
[0002] Monocrystalline silicon texturing technology is an important step in the production process of solar cells and is closely related to the development of solar cells. The working principle of solar cells is based on the absorption of light and the generation of electron-hole pairs, which in turn generate current.
[0003] The main purpose of texturing technology is to create microstructures on the surface of monocrystalline silicon through alkaline solution to reduce light reflection and increase light absorption. Specifically, texturing technology can form a series of tiny pyramidal or inverted pyramidal structures on the surface of silicon wafers. This structure has a high roughness and specific surface area, effectively increasing the contact area of light, allowing more light to enter the silicon body for interaction, enhancing the excitation of photogenerated carriers, thereby increasing short-circuit current and improving battery efficiency.
[0004] The process of preparing monocrystalline silicon cell includes texturing, diffusion, etching, coating, silk screen printing and other processes; the diffusion process is the core step of preparing PN junction and solar cell, and is greatly affected by process conditions and the previous texturing process; during the cutting process of silicon wafer, the cutting liquid and the adhesive rod are in direct contact with the silicon wafer, and organic matter and some metal impurities remain on the surface of the silicon wafer, mainly including the residues of elements such as C, O, Ca, and F. If the cleaning is not thorough, it will bring a series of adverse effects on the preparation of PN junction when it is brought into the high-temperature furnace tube. In addition to the contamination after the silicon wafer is cut, the residual texturing liquid, particles or organic matter will also cause the diffusion source to be unevenly distributed on the surface of the silicon wafer, and will also affect the diffusion depth, and the covering on the surface will increase the contact resistance of the battery, and the filling factor will decrease accordingly, which will affect the subsequent process and the performance of the battery; in addition, the particles or impurities that are not cleaned may cause defects on the surface of the silicon wafer, uneven velvet, white spots, leakage and other phenomena, resulting in local short circuit or open circuit, reducing the effective area and minority carrier life of the battery, causing poor EL, and reducing the efficiency and yield of the battery.
[0005] For the single crystal silicon raw wafers with serious contamination, including organic residues, positive and negative wafers, edge color difference and other appearance problems, they may affect the reaction between the texturing liquid and the silicon wafer surface; although some production lines usually perform rough polishing pre-treatment on this type of wafer source to achieve surface cleaning and mechanical damage layer treatment, improper treatment will still leave residues on the silicon wafer surface or cause new damage, which will have an adverse effect on the subsequent texturing and battery manufacturing process.
[0006] In addition to the rough polishing process, for single-crystal silicon wafers with heavy surface pollution, the production line process mainly relies on hydrogen peroxide and alkaline solutions to clean the surface organic matter and some metal ions to decompose the surface organic matter. For the production line, the large amount of hydrogen peroxide consumption is bound to bring a cost burden. By preparing a texturing additive with strong cleaning ability, it can not only remove the surface dirt, but also reduce the residue of the additive itself on the silicon wafer. At the same time, the dependence on hydrogen peroxide can be reduced to a certain extent, which can reduce the consumption of cleaning chemicals and increase the batches used for production line cleaning to achieve the purpose of improving production line efficiency and reducing consumption.
[0007] Therefore, it is of great significance to develop additives with strong cleaning capabilities. It can not only reduce the cleaning steps and time, reduce chemical consumption in the production process, improve the operating efficiency of the production line, and reduce production costs, but also effectively help stabilize the process and improve battery efficiency. Summary of the invention
[0008] The purpose of the present invention is to provide a monocrystalline silicon texturing additive and texturing method with strong contamination cleaning ability, which does not require a rough polishing process. Only one step of texturing can achieve the texturing and cleaning of a monocrystalline silicon wafer with severe contamination, and has the advantages of high stability, large window, strong cleaning ability, uniform velvet surface, etc. The dependence on the use of front and rear cleaning chemicals is reduced, the service life of the cleaning tank chemicals is extended, the chemical consumption in the production process is effectively reduced, and abnormal fluctuations in the production line and EL defects are reduced.
[0009] To solve the above technical problems, the purpose of the present invention is achieved as follows:
[0010] The present invention relates to a single crystal silicon texturing additive with strong contamination cleaning ability, comprising:
[0011]
[0012] On the basis of the above scheme and as a preferred scheme of the above scheme: the macromolecular sugar is: one or a combination of methyl cellulose, hydroxyethyl cellulose, carboxymethyl-B-cyclodextrin, gum arabic, colloid, sodium alginate.
[0013] Further preferred are methyl cellulose and carboxymethyl-B-cyclodextrin. The natural macromolecular sugars for the velvet surface are selected from one or two of carboxymethyl-B-cyclodextrin and methyl cellulose, both of which are polyhydroxy substances that can be adsorbed on the silicon wafer to form nucleation points as a mask to help form microstructures on the surface.
[0014] Since there are more dangling bonds on the Si(100) plane than on the Si(111) plane, the etching rate on the Si(100) plane is faster. Carboxymethyl-B-cyclodextrin is prepared by further modification of cyclodextrin. Since the hydroxyl groups are concentrated on the outside of the carboxymethyl-B-cyclodextrin molecule and the outer wall has strong hydrophilicity, it has strong adsorption capacity on the silicon (100) plane and forms a barrier layer on the surface of the single crystal silicon wafer. It has a strong blocking effect in the process of OH ions migrating from the etching solution to the silicon interface, which can delay the reaction and slow down the etching rate. This behavior is conducive to the stability of the texturing reaction process. On the other hand, carboxymethyl-B-cyclodextrin can increase the viscosity of the etching solution, and the structure of the hollow inner cavity for water delivery effectively separates the hydrogen bubbles attached to the silicon surface, increases the uniformity and coverage of the pyramids on the silicon surface, and effectively improves the size of the velvet caused by insufficient degassing.
[0015] On the basis of the above scheme and as a preferred scheme of the above scheme: the suede conditioning agent is: one or a combination of gelatin, polyvinyl alcohol, polyacrylamide or polyvinyl pyrrolidone.
[0016] On the basis of the above scheme and as a preferred scheme of the above scheme: the cleaning aid is: methacrylic acid-methyl acrylate copolymer, acrylic acid-allyl alcohol copolymer, allyl ether copolymer, sodium tripolyphosphate, sodium tetrapolyphosphate, sodium citrate or a combination of several thereof.
[0017] The further preferred cleaning aid is one or both of polyvinyl alcohol and polyvinyl pyrrolidone. The velvet conditioning agent is polyvinyl pyrrolidone and polyvinyl alcohol. The adsorption of macromolecular sugars on the surface of silicon wafers is unstable, and the pyramid size is too large, and the nucleation is not dense enough, resulting in high reflectivity and poor light capture ability, which needs to be further enhanced by the velvet conditioning agent; polyvinyl alcohol is also a type of hydrophilic polyhydroxy macromolecule, which can effectively form hydrogen bonds with silicon wafers, enhance the velvet removal efficiency and adjust the size to obtain a uniform and tiny size; polyvinyl pyrrolidone is an effective dispersant, because it carries different charges and the lonely electron structure on the N atom, it interacts with Si atoms on the silicon wafer surface through electrostatic action, adsorbs on the silicon wafer surface as a supplement, and synergizes with its macromolecular sugars to form a complete and uniform velvet with a high specific surface area.
[0018] On the basis of the above scheme and as a preferred scheme of the above scheme: the anionic surfactant is: one or a combination of several of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium stearate, and sodium stearoyl sarcosinate.
[0019] Further preferably, the cleaning aid is one or two of sodium tripolyphosphate, sodium citrate, etc., wherein sodium tripolyphosphate can form a cyclic complex with metal ions to reduce water hardness, and when combined with a phenotypic active agent, it greatly enhances the decontamination ability of silicon wafers.
[0020] On the basis of the above scheme and as a preferred scheme of the above scheme: the inorganic base is one or a combination of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium phosphate, and sodium acetate.
[0021] Further preferably, the anionic surfactant is one or both of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate. The sulfonic acid in sodium dodecylbenzene sulfonate protects the formed pyramid structure by combining with the dangling bonds on the (111) plane, and reduces the reaction rate by combining with the dangling bonds on the (100) plane, thereby ensuring that a uniform and dense pyramid structure is formed on the surface of the silicon wafer. That is, sodium dodecylbenzene sulfonate as a surfactant can effectively control the etching rate and adjust the pyramid size, so that the nucleation point is dense and uniform. At the same time, when compounded with other anionic surfactants, since the other end is a fatty chain, it has a certain dispersion of the velvet liquid, reduces the surface tension, and quickly desorbs the silicate on the surface of the silicon wafer to ensure the uniformity of the etching process. After the reaction is completed, the sulfonic acid group is close to the end surface of the silicon wafer and is attracted by van der Waals force. This loose connection can quickly take away the contamination and residual liquid of the silicon wafer, thereby ensuring the uniformity of the velvet surface and the cleanliness of the appearance of the silicon wafer.
[0022] The present invention also relates to a method for making single crystal silicon with strong contamination cleaning ability, comprising the following steps:
[0023] (1) Preparing a velvet-making additive: uniformly mixing natural macromolecular sugars, a velvet conditioning agent, a cleaning aid, a surfactant, an inorganic base and deionized water to prepare a velvet-making additive;
[0024] (2) preparing a texturing liquid: uniformly mixing the texturing additive prepared in the previous step with an alkali solution to prepare a texturing liquid;
[0025] (3) Texturing: Put the single crystal silicon wafer into a pure water pre-cleaning tank, add hydrogen peroxide and alkali; mix evenly, and then add texturing liquid to texturize the surface; after texturing, rinse with deionized water and dry to obtain the texturized silicon wafer.
[0026] The beneficial effects of the present invention are as follows: the present invention relates to a single crystal silicon texturing additive and texturing method with strong contamination cleaning ability, and the macromolecular sugar can be adsorbed on the silicon wafer to form nucleation points, which serve as a mask to help the surface form microstructures. The cleaning aid interacts with Si atoms on the silicon wafer surface through electrostatic action, and is adsorbed on the silicon wafer surface as a supplement, and synergizes with its macromolecular sugar to form a complete and uniform velvet surface with a high specific surface area. The anionic surfactant reduces the surface tension and quickly desorbs the silicate on the surface of the silicon wafer to ensure the uniformity of the etching process; after the reaction is completed, the sulfonic acid group is close to the end surface of the silicon wafer and is attracted by van der Waals force. This loose connection can quickly remove the contamination and residual liquid on the silicon wafer, ensuring the uniformity of the velvet surface and the cleanliness of the silicon wafer appearance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a SEM image of the suede prepared in Example 1;
[0028] Figure 2 is a SEM image of the suede prepared in Example 2;
[0029] Figure 3 This is the SEM image of the velvet prepared in Example 3. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0031] The present invention relates to a single crystal silicon texturing additive with strong contamination cleaning ability, comprising:
[0032]
[0033] Example 1
[0034] The present embodiment involves a method for texturing single crystal silicon with strong contamination cleaning capability, comprising the following steps:
[0035] (1) Preparation of texturing additives: According to a total of 100 parts, 1.0 part of methyl cellulose, 0.1 part of polyvinyl alcohol, 0.5 part of tripolyphosphoric acid, 0.09 part of sodium dodecylbenzene sulfonate, 1.0 part of inorganic alkali, and the rest of deionized water are uniformly mixed to prepare texturing additives.
[0036] (2) Preparation of texturing solution: First, prepare a 0.9 wt% NaOH solution in a texturing tank containing 20 L of pure water, then add the texturing additive in step (1) into the alkaline solution at a weight percentage of 0.5:100 and mix well. Then, bubble for 2 minutes to mix well to obtain the texturing solution.
[0037] (3) Texturing: Put a 182-size single crystal silicon wafer into a 20L pure water pre-cleaning tank, add hydrogen peroxide, sodium hydroxide and water in a mass percentage of 1.2:0.5:100 into the tank, bubbling for 2 minutes to mix evenly and perform surface texturing at a temperature of 82°C for 420 seconds. After texturing is completed, rinse the silicon wafer with a large amount of deionized water for 30 seconds and dry it to obtain the texturized silicon wafer.
[0038] Example 2
[0039] The present embodiment involves a method for texturing single crystal silicon with strong contamination cleaning capability, comprising the following steps:
[0040] (1) Preparation of texturing additives: According to a total of 100 parts, 1.0 part of methyl cellulose, 0.1 part of polyvinyl alcohol, 0.0 part of tripolyphosphoric acid, 0.0 part of sodium dodecylbenzene sulfonate, 1.0 part of inorganic alkali, and the rest of deionized water are uniformly mixed to prepare texturing additives.
[0041] (2) Preparation of texturing solution: First, prepare a 0.9 wt% NaOH solution in a texturing tank containing 20 L of pure water, then add the texturing additive in step (1) into the alkaline solution at a weight percentage of 0.5:100 and mix well. Then, bubble for 2 minutes to mix well to obtain the texturing solution.
[0042] (3) Texturing: Put a 182-size single crystal silicon wafer into a 20L pure water pre-cleaning tank, add hydrogen peroxide, sodium hydroxide and water in a mass percentage of 1.2:0.5:100 into the tank, bubbling for 2 minutes to mix evenly and perform surface texturing at a temperature of 82°C for 420 seconds. After texturing is completed, rinse the silicon wafer with a large amount of deionized water for 30 seconds and dry it to obtain the texturized silicon wafer.
[0043] Example 3
[0044] The present embodiment involves a method for texturing single crystal silicon with strong contamination cleaning capability, comprising the following steps:
[0045] (1) Preparation of texturing additives: According to a total of 100 parts, 1.2 parts of carboxymethyl-B-cyclodextrin, 0.15 parts of polyvinyl alcohol, 0.5 parts of tripolyphosphoric acid, 0.15 parts of sodium dodecylbenzene sulfonate, 1.0 parts of inorganic base, and the rest of deionized water are uniformly mixed to prepare the texturing additive.
[0046] (2) Preparation of texturing solution: First, prepare a 0.9 wt% NaOH solution in a texturing tank containing 20 L of pure water, then add the texturing additive in step (1) into the alkaline solution at a weight percentage of 0.5:100 and mix well. Then, bubble for 2 minutes to mix well to obtain the texturing solution.
[0047] (3) Texturing: Put a 182-size single crystal silicon wafer into a 20L pure water pre-cleaning tank, add hydrogen peroxide, sodium hydroxide and water in a mass percentage of 0.6:0.5:100 into the tank, bubbling for 2 minutes to mix evenly and perform surface texturing at a temperature of 82°C for 420 seconds. After texturing is completed, rinse the silicon wafer with a large amount of deionized water for 30 seconds and dry it to obtain the texturized silicon wafer.
[0048] Example 4
[0049] The present embodiment involves a method for texturing single crystal silicon with strong contamination cleaning capability, comprising the following steps:
[0050] (1) Preparation of texturing additives: According to a total of 100 parts, 2.0 parts of carboxymethyl-B-cyclodextrin, 0.08 parts of polyvinyl alcohol, 0.5 parts of tripolyphosphoric acid, 0.15 parts of sodium dodecylbenzene sulfonate, 1.0 parts of inorganic base, and the rest of deionized water are uniformly mixed to prepare the texturing additive.
[0051] (2) Preparation of texturing solution: First, prepare a 0.9 wt% NaOH solution in a texturing tank containing 20 L of pure water, then add the texturing additive in step (1) into the alkaline solution at a weight percentage of 0.5:100 and mix well. Then, bubble for 2 minutes to mix well to obtain the texturing solution.
[0052] (3) Texturing: Put a 182-size single crystal silicon wafer into a 20L pure water pre-cleaning tank, add hydrogen peroxide, sodium hydroxide and water in a mass percentage of 0.6:0.5:100 into the tank, bubbling for 2 minutes to mix evenly and perform surface texturing at a temperature of 82°C for 420 seconds. After texturing is completed, rinse the silicon wafer with a large amount of deionized water for 30 seconds and dry it to obtain the texturized silicon wafer.
[0053] Example 5
[0054] The present embodiment involves a method for texturing single crystal silicon with strong contamination cleaning capability, comprising the following steps:
[0055] (1) Preparation of texturing additives: According to a total of 100 parts, 0.8 parts of carboxymethyl-B-cyclodextrin, 0.5 parts of methyl cellulose, 0.05 parts of polyvinyl alcohol, 0.5 parts of tripolyphosphoric acid, 0.20 parts of sodium dodecylbenzene sulfonate, 1.0 parts of inorganic base, and the rest of deionized water are uniformly mixed to prepare the texturing additive.
[0056] (2) Preparation of texturing solution: First, prepare a 0.9 wt% NaOH solution in a texturing tank containing 20 L of pure water, then add the texturing additive in step (1) into the alkaline solution at a weight percentage of 0.5:100 and mix well. Then, bubble for 2 minutes to mix well to obtain the texturing solution.
[0057] (3) Texturing: Put a 182-size single crystal silicon wafer into a 20L pure water pre-cleaning tank, add hydrogen peroxide, sodium hydroxide and water in a mass percentage of 0.6:0.5:100 into the tank, bubbling for 2 minutes to mix evenly and perform surface texturing at a temperature of 82°C for 420 seconds. After texturing is completed, rinse the silicon wafer with a large amount of deionized water for 30 seconds and dry it to obtain the texturized silicon wafer.
[0058] The specific usage of each component in Examples 1 to 5 is shown in Table 1.
[0059]
[0060] Example 1 and Example 5 were tested, and the results are shown in Table 2.
[0061]
[0062] In the first embodiment, Figure 1 , a relatively complete suede surface can be obtained, and the appearance is clean, the pyramid size is 1.8um, and the reflectivity is 9.35%; while in Example 2, without the help of cleaning aids and surfactants, such as Figure 2 , the surface residue causes the failure of pyramid generation in the local area of the velvet surface or the incomplete pyramid morphology, which affects the structure size and uniformity of the pyramid, resulting in a high local reflectivity. The pyramid size and reflectivity are 1.3um and 10.02% respectively; it can be seen from Example 3 that after the amount of hydrogen peroxide used in the pre-cleaning is reduced by half, as shown in Figure 3 , it is still possible to obtain good results through one-step velveting on seriously contaminated sheets without residue on the surface, with pyramid size and reflectivity at 1.6um and 9.38%. Example 4 and Example 5 can still obtain uniform and complete velvet and good appearance under lower hydrogen peroxide conditions.
[0063] By testing the production line sample of the PERC cell manufacturer in Example 1, as shown in Table 3, an efficiency of 23.77% can be obtained, which can meet the needs of commercial production.
[0064]
[0065] Therefore, by adding cleaning aids and surfactants, a clean appearance with uniform color and a complete and dense velvet surface can be obtained through a one-step texturing process without rough polishing, and a good appearance and velvet surface can be obtained with a low amount of hydrogen peroxide, which successfully solves the texturing effect of the source of seriously polluted incoming materials, and is beneficial to the texturing process of seriously polluted materials without rough polishing. In addition, the consumption of hydrogen peroxide for cleaning can also be significantly reduced, and a good texturing effect can still be obtained.
[0066] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A single crystal silicon texturing additive with strong contamination cleaning ability, characterized in that: include:
2. The single crystal silicon texturing additive with strong contamination cleaning ability according to claim 1, characterized in that: The macromolecular sugar is one or a combination of methyl cellulose, hydroxyethyl cellulose, carboxymethyl-B-cyclodextrin, gum arabic, colloid, and sodium alginate.
3. The single crystal silicon texturing additive with strong contamination cleaning ability according to claim 1, characterized in that: The suede conditioning agent is one or a combination of gelatin, polyvinyl alcohol, polyacrylamide or polyvinyl pyrrolidone.
4. The single crystal silicon texturing additive with strong contamination cleaning ability according to claim 1, characterized in that: The cleaning aid is one or a combination of methacrylic acid-methyl acrylate copolymer, acrylic acid-allyl alcohol copolymer, allyl ether copolymer, sodium tripolyphosphate, sodium tetrapolyphosphate, and sodium citrate.
5. The single crystal silicon texturing additive with strong contamination cleaning ability according to claim 1, characterized in that: The anionic surfactant is one or a combination of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium stearate, and sodium stearoyl sarcosinate.
6. The single crystal silicon texturing additive with strong contamination cleaning ability according to claim 1, characterized in that: The inorganic base is one or a combination of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium phosphate and sodium acetate.
7. A method for texturing single crystal silicon with strong contamination cleaning capability, characterized in that: The steps include: (1) Preparing a velvet-making additive: uniformly mixing natural macromolecular sugars, a velvet conditioning agent, a cleaning aid, a surfactant, an inorganic base and deionized water to prepare a velvet-making additive; (2) preparing a texturing liquid: uniformly mixing the texturing additive prepared in the previous step with an alkali solution to prepare a texturing liquid; (3) Texturing: Put the single crystal silicon wafer into a pure water pre-cleaning tank, add hydrogen peroxide and alkali; mix evenly, and then add texturing liquid to texturize the surface; after texturing, rinse with deionized water and dry to obtain the texturized silicon wafer.
Citation Information
Cited By
IBC texturing additive suitable for N-type monocrystalline silicon wafer and use method of IBC texturing additive
CN121653855A