Low-pulling-speed direct rolling process of continuous casting machine

By adopting the low-pull-speed direct rolling process of continuous casting machines in steel production, real-time monitoring and controlling the process process, the problems of high energy consumption and inconsistent product quality in traditional processes are solved, and efficient and low-cost steel production is achieved.

CN119040732APending Publication Date: 2024-11-29SHANDONG IRON & STEEL GRP YONGFENG LINGANG CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411200308.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In traditional steel production processes, long-term operation of the heating furnace leads to high energy consumption and low production efficiency. The casting billet stays at high temperature for a long time and is prone to oxidation and segregation, which affects product quality and performance consistency.

Method used

Using the continuous casting machine's low-pull speed direct rolling process, the melting, refining, continuous casting, cutting, rolling and cooling process is monitored and controlled in real time, reducing the use time and pulling of the heating furnace, and directly rolling, optimizing cooling and straightening Treatment to reduce the degree of oxidation and segregation.

Benefits of technology

Significantly reduce energy consumption, improve production efficiency, reduce resource waste, improve product quality and performance consistency, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040732A_ABST
    Figure CN119040732A_ABST
Patent Text Reader

Abstract

The invention discloses a low-pulling-speed direct rolling process of a continuous casting machine, and relates to the technical field of steel production, the process comprises the following steps: S1, molten steel smelting: smelting raw materials in an electric furnace to obtain molten steel, strictly controlling the temperature, composition and impurity content in the smelting process, and accurately monitoring and adjusting the smelting process by adopting a real-time monitoring system; by shortening the service time of a heating furnace and reducing the pulling speed, the staying time of a casting blank at high temperature is shortened, the energy investment is greatly reduced, the production cost is reduced, the time and resource waste of intermediate links are reduced by shortening the technological process, and particularly, the casting blank can directly enter the direct rolling procedure after being cut, so that the production efficiency is improved. According to the method, cooling and reheating processes in a traditional process are avoided, the production efficiency is remarkably improved, low-pulling-speed direct rolling is adopted, the degree of oxidation and segregation is reduced, the microstructure of metal is improved, and the quality stability and consistency of products are effectively guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, in particular to a low-speed direct rolling process for a continuous casting machine. Background Art

[0002] The steel continuous casting machine is a metallurgical equipment that pours liquid steel directly into a water-cooled copper crystallizer, and finally obtains a solid ingot through a continuous cooling and solidification process. The high-temperature molten steel is continuously poured into one or a group of water-cooled copper crystallizers. The molten steel gradually solidifies into an ingot shell along the periphery of the crystallizer. When the steel liquid level rises to a certain height and the ingot shell solidifies to a certain thickness, the straightening machine pulls the ingot out and sprays water in the secondary cooling zone to completely solidify the ingot. Finally, the cutting device cuts it into fixed-length ingots according to the requirements of steel rolling. It is an important equipment in the steel production process. As an indispensable basic material in modern industry, the development of its production process is of vital importance to improving production efficiency, reducing costs, improving product quality and reducing environmental impact.

[0003] There are still some defects in the traditional steel production process. The heating furnace consumes a lot of energy during long-term operation, which increases the production cost. The traditional steel production process has multiple treatments after molten steel smelting, long-term cooling and reheating of the ingot, and other intermediate links, resulting in low production efficiency and serious waste of resources. Since the ingot stays at high temperature for a long time in the traditional process, it is easy to oxidize and segregate, which affects the microstructure of the metal and makes the mechanical properties of the product vary greatly. Therefore, it is necessary to propose a low-speed direct rolling process for continuous casting machines to solve the problems in the prior art. Summary of the invention

[0004] The purpose of the present invention is to make up for the shortcomings of the prior art and to provide a low-speed direct rolling process for a continuous casting machine. The low-speed direct rolling process can significantly reduce energy consumption, reduce the use time and energy input of the heating furnace, and reduce production costs. At the same time, it improves production efficiency, shortens the process flow, and reduces time and resource waste in the intermediate links. The low-speed direct rolling process reduces the residence time of the ingot at high temperature, reduces the degree of oxidation and segregation, and thus improves the quality and performance consistency of the product.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a low-speed direct rolling process of a continuous casting machine, the process comprising the following steps: S1. Molten steel smelting: The raw materials are smelted in an electric furnace to obtain molten steel. The temperature, composition and impurity content during the smelting process are strictly controlled, and a real-time monitoring system is used to accurately monitor and adjust the smelting process; S2. Refining treatment: Refining the molten steel after melting, using vacuum degassing and argon blowing and stirring to remove impurities and adjust the composition, and controlling the vacuum degree within a specific range; S3, continuous casting: inject the molten steel into the continuous casting machine for continuous casting to form a cast billet. Control the casting speed during the continuous casting process to less than 70% of the traditional casting speed and optimize the cooling system of the crystallizer. S4, billet cutting: cutting the continuously cast billet into predetermined lengths; S5, direct rolling: the ingot is directly rolled into the rolling mill without long-term cooling and reheating; S6, Intermediate cooling: During the rolling process, intermediate cooling is carried out according to product requirements to control the cooling speed and cooling uniformity; S7, finishing: Finishing of rolled products, including cutting, straightening, and flaw detection; S8. Finished product inspection: Conduct a comprehensive quality inspection on the finished products, including chemical composition analysis, mechanical properties testing, and surface defect detection, and determine whether the products are qualified based on strict quality standards.

[0006] Furthermore, the specific steps of S1, molten steel smelting, include: Accurately calculate and prepare various raw materials, including iron ore, scrap steel, and alloying elements, according to the composition requirements of the required steel grades; The screened and weighed raw materials are loaded into the electric furnace in a certain order and proportion; Start the electric furnace heating device to gradually increase the temperature in the furnace and promote the melting of the raw materials; As the raw materials melt, slag-forming agents are added in time to form slag, and the slag-steel reaction is promoted through stirring and blowing operations; Use online testing equipment to monitor the composition of molten steel in real time, and add alloy elements to fine-tune the composition according to the test results to make the composition of molten steel reach the specified range; Continuously monitor the temperature of the molten steel and control it within an appropriate range by adjusting the heating power and adding coolant; Comprehensively consider the composition, temperature and purity of the molten steel to accurately determine the smelting end point.

[0007] Furthermore, the specific steps of the refining process in S2 include: Use special ladles and transfer equipment to transfer the molten steel to the refining furnace; The refining furnace is evacuated to control the vacuum degree within a specific range, so that the gas dissolved in the molten steel can escape under the vacuum environment; Inject argon into the molten steel to make the composition and temperature of the molten steel more uniform, and control the flow rate and injection depth of argon; According to the composition test results of molten steel, alloy elements are added and fine-tuned again; Desulfurizing agents, including lime and magnesium powder, are added to react with sulfur in the molten steel to form sulfides that float up and are removed. Inclusions in the molten steel are further removed by slagging and adsorption; Monitor the temperature of molten steel, comprehensively consider the composition, temperature, purity and inclusion content of molten steel, accurately determine the end point of refining treatment, and use a combination of advanced detection technology and experience judgment to optimize the quality of refined molten steel.

[0008] Furthermore, the specific steps of S3, continuous casting include: The refined molten steel is hoisted into the ladle of the continuous casting machine, and the molten steel is subjected to final composition and temperature testing to confirm that it meets the requirements of continuous casting; Clean and preheat the tundish to reach the predetermined temperature, reduce the heat loss of the molten steel and prevent the molten steel from solidifying in the tundish, install the immersion nozzle and stopper flow control device of the tundish, and conduct inspection and commissioning; Check and clean the crystallizer, install the cooling device of the crystallizer, and adjust the cooling water flow rate and water temperature; Open the water inlet of the ladle and slowly inject the molten steel into the tundish. Through the flow control device of the tundish, the molten steel flows into the crystallizer evenly and stably. The molten steel contacts the inner wall of the mold and begins to solidify to form a thin shell, which controls the vibration frequency and amplitude of the mold, helps demoulding and improves the surface quality of the ingot; Start the billet drawing machine and pull the billet out of the crystallizer at a set low pulling speed, with the pulling speed controlled below 70% of the conventional pulling speed; After the billet leaves the crystallizer, it passes through the secondary cooling section, where it is further cooled by water spray and mist cooling. The cooling nozzles are arranged reasonably to control the cooling intensity and uniformity to prevent cracks in the billet. When the ingot reaches a certain strength, the ingot is straightened by a straightening device to eliminate the bending of the ingot.

[0009] Furthermore, the specific steps of S4, cutting the ingot, include: According to the predetermined length, the ingot is cut by cutting equipment. First, the working status of the cutting equipment is checked, and the equipment is preheated and debugged as necessary; The continuous casting billet is accurately transported to the cutting station and fixed by the positioning device; Set the relevant parameters of the cutting equipment according to the specifications and materials of the ingot and the predetermined cutting length; The operator starts the cutting equipment and the cutter begins to cut the ingot; Use automatic control system and manual intervention to adjust cutting parameters; After cutting is completed, the cut surface is inspected to check whether the flatness, verticality and dimensional accuracy of the cut surface meet the requirements; Collect and process the waste generated by cutting and store it in categories; The qualified ingots are transported to the direct rolling process through the conveying device.

[0010] Furthermore, the specific steps of S5, direct rolling, include: Re-check the cut and delivered ingots to confirm that the surface quality, size and temperature of the ingots meet the requirements of direct rolling; Start the rolling mill in advance and preheat the main parts of the rolling mill to reach the appropriate working temperature, and control the uniformity of the preheating temperature; According to product specifications and performance requirements, set various process parameters of the rolling mill, referring to previous process data and simulation results; The prepared ingot is smoothly introduced into the rolling mill, and the ingot introduction position is monitored in real time using guide devices and sensors.

[0011] Furthermore, the specific steps of S5, direct rolling, also include: Start the first rolling pass to make the ingot deform initially, monitor the rolling force and torque parameters, and adjust the parameters in time to ensure the stability of rolling; According to the set rolling passes and parameters, the ingot is rolled step by step for multiple passes. During the rolling process, the shape, size and internal structure of the ingot are tested online. According to the rolling process and the temperature change of the ingot, appropriate heating and cooling measures are adopted to control the temperature of the ingot within a reasonable range; Real-time measurement of the size of the billet after rolling, fine-tuning the rolling mill parameters based on the measurement results to ensure product dimensional accuracy; Complete the last rolling pass to make the ingot reach the predetermined shape, size and performance requirements, and conduct a comprehensive inspection of the final rolled product; The rolled products are output from the rolling mill and sent to subsequent processes through a conveying device.

[0012] Furthermore, the specific steps of S6, intermediate cooling, include: During the rolling process, the temperature, deformation degree and changes in the metal structure of the ingot are monitored in real time. According to the product specifications and performance requirements, as well as the previously set process parameters, it is determined whether intermediate cooling is required and the degree of cooling; Based on the evaluation results, determine the cooling method to be adopted, including mist cooling and water spray cooling; Set the relevant parameters of the cooling system, including the flow rate, pressure, and temperature of the cooling medium, and determine the length, width, and cooling time of the cooling area; Start the cooling system so that the cooling medium acts on the ingot according to the set parameters; During the cooling process, a temperature sensor is used to monitor the temperature change of the ingot in real time and observe the spraying of the cooling medium; Based on the monitored temperature data and the surface condition of the ingot, evaluate whether the cooling effect meets expectations; When the ingot reaches the predetermined cooling temperature and meets the process requirements, cooling is stopped.

[0013] Furthermore, the specific steps of S7, finishing include: Measure the rolled product to determine the exact location where it needs to be cut, and use the cutting equipment to cut it to the predetermined length; The cut products are straightened by a straightening machine. According to the material and specifications of the products, the pressure, roller distance and straightening speed of the straightening machine are adjusted, and the straightness of the straightened products is checked in real time. Use grinding and polishing methods to remove oxide scale, scratches and minor defects on the product surface; Use non-destructive testing technology to detect defects inside and on the surface of products; Use calipers and micrometers to make detailed measurements of product dimensions and compare the measurement results with design requirements; Take some products for mechanical property testing, analyze the test results, and verify whether the strength and toughness of the products meet the use requirements; Based on the results of the above inspections and tests, the products are graded for quality, qualified products and unqualified products are classified and stored, unqualified products are marked and recorded, and qualified products are packaged.

[0014] Furthermore, the specific steps of S8, finished product inspection include: Comprehensively observe the appearance of the finished product to check whether there are cracks, pits, scratches, rust spots or other defects on the surface; Use high-precision measuring tools to accurately measure the key dimensions of length, width, thickness and diameter of the finished product, and compare the measurement results with the dimensional tolerances specified in the product design drawings and relevant standards; Use spectral analysis and chemical analysis to detect the content of various chemical components in the finished product, focusing on whether the content of major alloy elements and harmful impurity elements meets product requirements and relevant standards; Take samples from the finished product for tensile testing to determine the mechanical properties of yield strength, tensile strength and elongation, and conduct hardness testing to evaluate the hardness level of the finished product; For products with special requirements, magnetic properties, electrical properties and thermal conductivity tests are carried out; Observe the microstructure of the finished product through a metallographic microscope to assess whether the microstructure is uniform and dense, and whether there are any abnormal structures; Conduct non-destructive testing review on products that have undergone flaw detection in the finishing stage; According to the above test results, comprehensively determine the quality level of the finished product, record the test data and results in detail, establish a quality file, and provide a basis for quality traceability; For products that fail the inspection, the type and reason of the failure shall be clearly stated.

[0015] Compared with the existing technology, the low-speed direct rolling process of the continuous casting machine has the following beneficial effects: The present invention reduces the use time of the heating furnace and the drawing speed, thereby reducing the residence time of the ingot at high temperature, greatly reducing energy input and reducing production costs. It shortens the process flow and reduces the waste of time and resources in the intermediate links. In particular, the ingot can directly enter the direct rolling process after cutting, avoiding the cooling and reheating process in the traditional process, and achieving a significant improvement in production efficiency. The low drawing speed direct rolling is used to reduce the degree of oxidation and segregation, improve the microstructure of the metal, and effectively ensure the quality stability and consistency of the product.

[0016] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 The figure is a process flow chart of a low-speed direct rolling process of a continuous casting machine. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Embodiment 1 A low-drawing speed direct rolling process for a continuous casting machine comprises the following steps: firstly, raw materials are smelted in an electric furnace to obtain molten steel that meets the requirements, the temperature, composition and impurity content during the smelting process are strictly controlled, and the smelting process is accurately monitored and adjusted by a real-time monitoring system, then the smelted molten steel is refined, vacuum degassing and argon blowing and stirring are used to remove impurities and adjust the composition, the vacuum degree is controlled within a specific range, and then the smelted molten steel is injected into a continuous casting machine for continuous casting to form a cast billet, the drawing speed during the continuous casting process is controlled to be less than 70% of the traditional drawing speed, and the cooling system of the crystallizer is optimized.

[0021] Next, the continuously cast ingot is cut into predetermined lengths, and high-precision cutting equipment is used to ensure the flatness and dimensional accuracy of the cut surface. The ingot is directly rolled into the rolling mill without long-term cooling and reheating. The process parameters of the rolling mill are optimized, and an advanced rolling control system is configured. During the rolling process, intermediate cooling is performed according to product requirements, and the cooling rate and cooling uniformity are controlled. The rolled products are subjected to finishing treatment, including cutting, straightening, and flaw detection, using advanced finishing equipment and technology. Finally, the finished products are subjected to comprehensive quality inspection, including chemical composition analysis, mechanical property testing, and surface defect detection, and the qualification of the products is determined according to strict quality standards.

[0022] In this embodiment, the process reduces the use time of the heating furnace and lowers the drawing speed, reduces the residence time of the ingot at high temperature, greatly reduces energy input, and reduces production costs. By shortening the process flow, the time and resource waste in the intermediate links are reduced. In particular, the ingot can directly enter the direct rolling process after cutting, avoiding the cooling and reheating process in the traditional process, and achieving a significant improvement in production efficiency. The use of low drawing speed direct rolling reduces the degree of oxidation and segregation, improves the microstructure of the metal, and effectively guarantees the quality stability and consistency of the product.

[0023] Embodiment 2 This embodiment further describes the embodiment 1 in detail. The specific working process of a low-speed direct rolling process of a continuous casting machine includes: First, according to the composition requirements of the required steel grade, various raw materials, including iron ore, scrap steel, and alloy elements, are accurately calculated and prepared. The raw materials are strictly quality tested to ensure that their purity and impurity content meet the requirements. For example, for scrap steel, its chemical composition and physical state should be checked, and the parts that do not meet the standards should be removed. The screened and weighed raw materials should be loaded into the electric furnace in a certain order and proportion. During the loading process, attention should be paid to uniform distribution to ensure the uniformity of heating and reaction in the furnace. The electric furnace heating device is started to gradually increase the temperature in the furnace to promote the melting of the raw materials. The heating speed and temperature curve are strictly controlled to avoid adverse effects on the quality of the molten steel due to excessively high or low temperatures. For example, a lower power is used for preheating in the early stage, and then the power is gradually increased to speed up the melting speed. As the raw materials melt, slag-forming agents are added in time to form slag to remove impurities such as phosphorus in the molten steel.

[0024] Then, through stirring and blowing operations, the slag-steel reaction is promoted to improve the dephosphorization effect. The online detection equipment is used to monitor the composition of the molten steel in real time. According to the test results, alloy elements are added to fine-tune the composition so that the composition of the molten steel reaches the specified range. For example, when the carbon content is detected to be insufficient, an appropriate amount of carbonaceous material is accurately added. The molten steel temperature is continuously monitored and the molten steel temperature is controlled within an appropriate range by adjusting the heating power and adding coolant to ensure that the molten steel temperature meets the requirements of subsequent processes and does not lead to excessive oxidation and energy waste due to being too high. The composition, temperature and purity of the molten steel are comprehensively considered to accurately determine the smelting end point. A combination of advanced detection technology and experience judgment is used to ensure that the quality of the molten steel meets the requirements for entering the next process.

[0025] Next, a special ladle and transfer equipment are used to carefully transfer the smelted molten steel to the refining furnace to ensure that the temperature loss and secondary oxidation of the molten steel are minimized during the transfer process to ensure the smooth transportation of the molten steel. The refining furnace is evacuated and the vacuum degree is controlled within a specific range, usually below 100Pa. In a vacuum environment, the gases dissolved in the molten steel (such as hydrogen, nitrogen, etc.) are encouraged to escape, reducing the gas content in the steel and improving the purity of the molten steel. Argon is introduced into the molten steel. Through the stirring effect of argon, the composition and temperature of the molten steel are made more uniform. The flow rate and blowing depth of argon are controlled to achieve the best stirring effect and promote the floating and removal of inclusions.

[0026] Then, according to the test results of the composition of the molten steel, the alloying elements are added and fine-tuned again, and the amount of the required alloying elements added is accurately calculated to ensure that the composition of the molten steel accurately meets the product requirements. Desulfurizers, including lime and magnesium powder, are added to react with the sulfur in the molten steel to form sulfides and float up for removal. The amount of desulfurizer added and the reaction time are controlled to achieve the ideal desulfurization effect. The inclusions in the molten steel are further removed by slag making and adsorption. The composition and properties of the slag are adjusted to improve its ability to adsorb inclusions. The temperature of the molten steel is monitored. If necessary, the temperature of the molten steel is adjusted to a range suitable for the subsequent continuous casting process by heating or cooling to ensure the stability and uniformity of the molten steel temperature. The composition, temperature, purity, and inclusion content of the molten steel are comprehensively considered to accurately determine the end point of the refining treatment. A combination of advanced detection technology and experience judgment is used to optimize the quality of the refined molten steel. In the entire refining process, the above steps are strictly implemented and closely coordinated with the previous and subsequent processes, which can significantly improve the quality of the molten steel and provide a good foundation for subsequent continuous casting, direct rolling and other processes.

[0027] Next, the refined molten steel is hoisted into the ladle of the continuous casting machine to ensure that the temperature and composition of the molten steel are stable during transportation. The molten steel is finally tested for composition and temperature to confirm that it meets the requirements of continuous casting. The tundish is cleaned and preheated to reach the predetermined temperature to reduce the heat loss of the molten steel and prevent the molten steel from solidifying in the tundish. The immersion nozzle and stopper rod flow control device of the tundish are installed, and then inspected and debugged. The crystallizer is inspected and cleaned to ensure that the inner wall is smooth and undamaged. The cooling device of the crystallizer is installed, and the cooling water flow rate and water temperature are debugged to ensure a good cooling effect. The water nozzle of the ladle is opened, and the molten steel is slowly injected into the tundish. The molten steel is made to flow into the crystallizer evenly and stably through the flow control device of the tundish. The molten steel contacts the inner wall in the crystallizer and begins to solidify to form a thin shell. The vibration frequency and amplitude of the crystallizer are controlled to help demoulding and improve the surface quality of the ingot. Then, start the billet drawing machine and pull the billet out of the crystallizer at a set low pulling speed. The pulling speed is controlled below 70% of the traditional pulling speed to reduce the residence time of the billet at high temperature. After the billet leaves the crystallizer, it passes through the secondary cooling section and is further cooled by water spray and mist cooling. The cooling nozzles are arranged reasonably, and the cooling intensity and uniformity are controlled to prevent cracks in the billet. When the billet reaches a certain strength, the billet is straightened by the straightening device to eliminate the bending of the billet, and the straightening force and straightening temperature are controlled to avoid damage to the billet. During the entire continuous casting process, the above steps are strictly followed and various parameters such as pulling speed, cooling intensity, temperature, etc. are closely monitored. According to the predetermined length, the ingot is cut by cutting equipment to ensure that the cutting surface is flat and the dimensional accuracy meets the requirements. First, check the working status of the cutting equipment, including the wear of the tool and whether the drive device is operating normally, to ensure that the accuracy and stability of the cutting equipment meet the requirements, and perform necessary preheating and debugging on the equipment. The ingot completed by continuous casting is accurately transported to the cutting station and fixed by a positioning device to ensure that the ingot will not move during the cutting process to ensure the accuracy of the cutting size. According to the specifications and material of the ingot and the predetermined cutting length, set the relevant parameters of the cutting equipment, for example, determine the cutting speed, cutting pressure, tool feed rate and other parameters.

[0028] The operator starts the cutting equipment, and the tool begins to cut the ingot. During the cutting process, the cutting process is monitored in real time to observe whether there are any abnormal conditions, such as excessive sparks, uneven cutting surfaces, etc. The automatic control system and manual intervention are used to adjust the cutting parameters to ensure the cutting quality. For example, the cutting speed is adjusted in time according to the temperature change of the ingot to prevent the cutting quality from being reduced due to the ingot temperature being too high or too low. After the cutting is completed, the cut surface is inspected to check whether the flatness, verticality and dimensional accuracy of the cut surface meet the requirements. If any part that does not meet the requirements is found, it is marked and recorded in time, and the waste generated by the cutting is collected and processed, and stored in categories for subsequent recycling or proper disposal. The ingots that have passed the cutting are conveyed to the direct rolling process through the conveying device. During the entire process of ingot cutting, the above steps are strictly followed, and flexible adjustments and optimizations are made according to actual conditions.

[0029] Recheck the cut and delivered ingots to confirm that the surface quality, size and temperature of the ingots meet the requirements of direct rolling. If necessary, clean up the minor defects on the surface of the ingots. Start the rolling mill in advance and preheat the main components of the rolling mill (rollers, etc.) to reach a suitable working temperature. Control the uniformity of the preheating temperature to avoid local overheating or overcooling. Set the various process parameters of the rolling mill, such as rolling speed, rolling passes, reduction, etc., according to product specifications and performance requirements. Refer to previous process data and simulation results to ensure the rationality of the parameters. Smoothly guide the prepared ingots into the rolling mill to ensure accurate alignment of the ingots and rolls. Use guide devices and sensors to monitor the introduction position of the ingots in real time.

[0030] The first rolling pass is started to make the ingot initially deformed, the rolling force and torque parameters are monitored, and the parameters are adjusted in time to ensure the stability of rolling. According to the set rolling passes and parameters, the ingot is gradually rolled for multiple passes. During the rolling process, the shape, size and internal structure of the ingot are detected online. According to the rolling progress and the temperature change of the ingot, appropriate heating and cooling measures are adopted to control the temperature of the ingot within a reasonable range. For example, induction heating or spray cooling is used to ensure that the temperature of the ingot is uniform and meets the requirements of metal deformation. The size of the ingot after rolling is measured in real time, and the rolling mill parameters are fine-tuned according to the measurement results to ensure the dimensional accuracy of the product. High-precision measuring instruments, such as laser thickness gauges, profilometers, etc., are used to complete the last rolling pass so that the ingot meets the predetermined shape, size and performance requirements. The product after final rolling is fully tested, including surface quality, dimensional accuracy, mechanical properties, etc. The rolled product is output from the rolling mill and sent to the subsequent process through a conveying device.

[0031] During the entire process of direct rolling, the above steps are strictly followed and combined with advanced detection and control technologies to ensure the stability and efficiency of the direct rolling process.

[0032] During the rolling process, the temperature, deformation degree and changes in the metal structure of the ingot are monitored in real time. According to the product specifications and performance requirements, as well as the previously set process parameters, it is determined whether intermediate cooling is required and the degree of cooling. According to the evaluation results, the cooling method to be adopted is determined, including mist cooling and water spray cooling. For example, if the cooling uniformity requirement is high, mist cooling is selected; if rapid cooling is required, water spray cooling may be selected. The relevant parameters of the cooling system are set, including the flow rate, pressure and temperature of the cooling medium. At the same time, the length, width and cooling time of the cooling area are determined, and the cooling system is started so that the cooling medium acts on the ingot according to the set parameters to ensure that the cooling medium is sprayed evenly and covers the entire area to be cooled. During the cooling process, the temperature sensor is used to monitor the temperature change of the ingot in real time, and the spraying of the cooling medium is observed. If there is blockage or unevenness, it is adjusted in time. According to the monitored temperature data and the surface state of the ingot, it is evaluated whether the cooling effect meets the expectations; if it does not meet the expectations, the cooling parameters are adjusted in time or supplementary cooling measures are taken. When the ingot reaches the predetermined cooling temperature and meets the process requirements, the cooling is stopped to ensure that the cooling is completed accurately to avoid excessive cooling or insufficient cooling.

[0033] During the entire process of intermediate cooling, the above steps are strictly followed and closely coordinated with other direct rolling processes.

[0034] Then, measure the rolled product to determine the exact location where cutting is required, use high-precision cutting equipment, such as laser cutting machine or plasma cutting machine, to cut according to the predetermined length, ensure that the length error of the cut product is within the allowable range, straighten the cut product through a straightener, adjust the pressure, roller distance and straightening speed of the straightener according to the material and specifications of the product, check the straightness of the straightened product in real time to ensure that it meets the quality standards, use grinding and polishing methods to remove oxide scale, scratches and minor defects on the product surface, and for products with higher requirements, pickling or sand blasting can be performed to obtain a smooth surface.

[0035] Next, use non-destructive testing techniques, such as ultrasonic testing and magnetic particle testing, to detect defects inside and on the surface of the product. Mark and evaluate the detected defects to determine whether they are within an acceptable range. Use calipers and micrometers to measure the dimensions of the product (including length, width, thickness, etc.) in detail. Compare the measurement results with the design requirements to ensure that the dimensional accuracy meets the standards. Take some products for mechanical property tests, such as tensile tests and hardness tests. Analyze the test results to verify whether the strength and toughness of the products meet the use requirements. According to the results of the above inspections and tests, grade the products by quality, classify qualified and unqualified products, and mark and record the unqualified products. Package qualified products using rust-proof and moisture-proof packaging materials to protect the products from damage during transportation and storage.

[0036] During the entire finishing process, the above steps are strictly followed and advanced equipment and testing methods are used to ensure that the quality and performance of the products are in the best condition.

[0037] Finally, the appearance of the finished product is comprehensively observed to check whether there are cracks, pits, scratches, rust spots on the surface. Lighting equipment and magnifying glass tools are used to ensure that subtle surface defects can also be found. High-precision measuring tools such as calipers, micrometers, and diameter gauges are used to accurately measure the key dimensions of the length, width, thickness, and diameter of the finished product. The measurement results are compared with the dimensional tolerances specified in the product design drawings and relevant standards. Spectroscopic analysis and chemical analysis methods are used to detect the content of various chemical components in the finished product, focusing on whether the content of major alloying elements and harmful impurity elements meets product requirements and relevant standards. Samples are taken from the finished product for testing. Conduct tensile tests to determine the mechanical properties of yield strength, tensile strength and elongation; perform hardness tests, such as Brinell hardness and Rockwell hardness, to evaluate the hardness level of the finished product; for products with special requirements, conduct magnetic, electrical and thermal conductivity tests to ensure that the physical properties meet the specific usage scenarios and needs of the product; observe the microstructure of the finished product through a metallographic microscope, including grain size, morphology, phase composition, etc., to evaluate whether the microstructure is uniform and dense, and whether there are any abnormal structures; conduct non-destructive testing and review of products that have undergone flaw detection in the finishing stage to ensure that no new internal defects are generated; ultrasonic flaw detection, X-ray flaw detection and other methods may be used.

[0038] Finally, based on the above test results, the quality grade of the finished product is comprehensively determined, the test data and results are recorded in detail, and a quality file is established to provide a basis for quality traceability. For products that fail the inspection, the type and cause of the failure are clarified. Depending on the specific situation, measures such as rework, scrapping or downgrading are taken, and the processing process and results are recorded. During the entire process of finished product inspection, the above steps are strictly followed and judgments are made based on strict quality standards.

[0039] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the same elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A low-speed direct rolling process for a continuous casting machine, characterized in that: The process includes the following steps: S1. Molten steel smelting: The raw materials are smelted in an electric furnace to obtain molten steel. The temperature, composition and impurity content during the smelting process are strictly controlled, and a real-time monitoring system is used to accurately monitor and adjust the smelting process; S2. Refining treatment: Refining the molten steel after melting, using vacuum degassing and argon blowing and stirring to remove impurities and adjust the composition, and controlling the vacuum degree within a specific range; S3, continuous casting: inject the molten steel into the continuous casting machine for continuous casting to form a cast billet. Control the casting speed during the continuous casting process to less than 70% of the traditional casting speed and optimize the cooling system of the crystallizer. S4, billet cutting: cutting the continuously cast billet into predetermined lengths; S5, direct rolling: the ingot is directly rolled into the rolling mill without long-term cooling and reheating; S6, Intermediate cooling: During the rolling process, intermediate cooling is carried out according to product requirements to control the cooling speed and cooling uniformity; S7, finishing: Finishing of rolled products, including cutting, straightening, and flaw detection; S8. Finished product inspection: Conduct a comprehensive quality inspection on the finished products, including chemical composition analysis, mechanical properties testing, and surface defect detection, and determine whether the products are qualified based on strict quality standards.

2. A continuous casting machine low-speed direct rolling process according to claim 1, characterized in that: The specific steps of S1, molten steel smelting include: Accurately calculate and prepare various raw materials, including iron ore, scrap steel, and alloying elements, according to the composition requirements of the required steel grades; The screened and weighed raw materials are loaded into the electric furnace in a certain order and proportion; Start the electric furnace heating device to gradually increase the temperature in the furnace and promote the melting of the raw materials; As the raw materials melt, slag-forming agents are added in time to form slag, and the slag-steel reaction is promoted through stirring and blowing operations; Use online testing equipment to monitor the composition of molten steel in real time, and add alloy elements to fine-tune the composition according to the test results to make the composition of molten steel reach the specified range; Continuously monitor the temperature of the molten steel and control it within an appropriate range by adjusting the heating power and adding coolant; Comprehensively consider the composition, temperature and purity of the molten steel to accurately determine the smelting end point.

3. A continuous casting machine low-speed direct rolling process according to claim 1, characterized in that: The specific steps of the refining process in S2 include: Use special ladles and transfer equipment to transfer the molten steel to the refining furnace; The refining furnace is evacuated to control the vacuum degree within a specific range, so that the gas dissolved in the molten steel can escape under the vacuum environment; Inject argon into the molten steel to make the composition and temperature of the molten steel more uniform, and control the flow rate and injection depth of argon; According to the composition test results of molten steel, alloy elements are added and fine-tuned again; Desulfurizing agents, including lime and magnesium powder, are added to react with sulfur in the molten steel to form sulfides that float up and are removed. Inclusions in the molten steel are further removed by slagging and adsorption; Monitor the temperature of molten steel, comprehensively consider the composition, temperature, purity and inclusion content of molten steel, accurately determine the end point of refining treatment, and use a combination of advanced detection technology and experience judgment to optimize the quality of refined molten steel.

4. A continuous casting machine low-speed direct rolling process according to claim 1, characterized in that: The specific steps of S3, continuous casting, include: The refined molten steel is hoisted into the ladle of the continuous casting machine, and the molten steel is subjected to final composition and temperature testing to confirm that it meets the requirements of continuous casting; Clean and preheat the tundish to reach the predetermined temperature, reduce the heat loss of the molten steel and prevent the molten steel from solidifying in the tundish, install the immersion nozzle and stopper flow control device of the tundish, and conduct inspection and commissioning; Check and clean the crystallizer, install the cooling device of the crystallizer, and adjust the cooling water flow rate and water temperature; Open the water inlet of the ladle and slowly inject the molten steel into the tundish. Through the flow control device of the tundish, the molten steel flows into the crystallizer evenly and stably. The molten steel contacts the inner wall of the mold and begins to solidify to form a thin shell, which controls the vibration frequency and amplitude of the mold, helps demoulding and improves the surface quality of the ingot; Start the billet drawing machine and pull the billet out of the crystallizer at a set low pulling speed, with the pulling speed controlled below 70% of the conventional pulling speed; After the billet leaves the crystallizer, it passes through the secondary cooling section, where it is further cooled by water spray and mist cooling. The cooling nozzles are arranged reasonably to control the cooling intensity and uniformity to prevent cracks in the billet. When the ingot reaches a certain strength, the ingot is straightened by a straightening device to eliminate the bending of the ingot.

5. The low-speed direct rolling process of a continuous casting machine according to claim 1, characterized in that: The specific steps of S4, cutting the ingot, include: According to the predetermined length, the ingot is cut by cutting equipment. First, the working status of the cutting equipment is checked, and the equipment is preheated and debugged as necessary; The continuous casting billet is accurately transported to the cutting station and fixed by the positioning device; Set the relevant parameters of the cutting equipment according to the specifications and materials of the ingot and the predetermined cutting length; The operator starts the cutting equipment and the cutter begins to cut the ingot; Use automatic control system and manual intervention to adjust cutting parameters; After cutting, the cutting surface is inspected to check whether the flatness, verticality and dimensional accuracy of the cutting surface meet the requirements; Collect and process the waste generated by cutting and store it in categories; The qualified ingots are transported to the direct rolling process through the conveying device.

6. A continuous casting machine low-speed direct rolling process according to claim 1, characterized in that: The specific steps of S5, direct rolling, include: Re-check the cut and delivered ingots to confirm that the surface quality, size and temperature of the ingots meet the requirements of direct rolling; Start the rolling mill in advance and preheat the main parts of the rolling mill to reach the appropriate working temperature, and control the uniformity of the preheating temperature; According to product specifications and performance requirements, set various process parameters of the rolling mill, referring to previous process data and simulation results; The prepared ingot is smoothly introduced into the rolling mill, and the ingot introduction position is monitored in real time using the guide device and sensors.

7. A continuous casting machine low-speed direct rolling process according to claim 6, characterized in that: The specific steps of S5, direct rolling, also include: Start the first rolling pass to make the ingot deform initially, monitor the rolling force and torque parameters, and adjust the parameters in time to ensure the stability of rolling; According to the set rolling passes and parameters, the ingot is rolled step by step for multiple passes. During the rolling process, the shape, size and internal structure of the ingot are tested online. According to the rolling process and the temperature change of the ingot, appropriate heating and cooling measures are adopted to control the temperature of the ingot within a reasonable range; Real-time measurement of the size of the billet after rolling, fine-tuning the rolling mill parameters based on the measurement results to ensure product dimensional accuracy; Complete the last rolling pass to make the ingot reach the predetermined shape, size and performance requirements, and conduct a comprehensive inspection of the final rolled product; The rolled products are output from the rolling mill and sent to subsequent processes through a conveying device.

8. The low-speed direct rolling process of a continuous casting machine according to claim 1, characterized in that: The specific steps of S6, intermediate cooling, include: During the rolling process, the temperature, deformation degree and changes in the metal structure of the ingot are monitored in real time. According to the product specifications and performance requirements, as well as the previously set process parameters, it is determined whether intermediate cooling is required and the degree of cooling; Based on the evaluation results, determine the cooling method to be adopted, including mist cooling and water spray cooling; Set the relevant parameters of the cooling system, including the flow rate, pressure, and temperature of the cooling medium, and determine the length, width, and cooling time of the cooling area; Start the cooling system so that the cooling medium acts on the ingot according to the set parameters; During the cooling process, a temperature sensor is used to monitor the temperature change of the ingot in real time and observe the spraying of the cooling medium; Based on the monitored temperature data and the surface condition of the ingot, evaluate whether the cooling effect meets expectations; When the ingot reaches the predetermined cooling temperature and meets the process requirements, cooling is stopped.

9. A continuous casting machine low-speed direct rolling process according to claim 1, characterized in that: The specific steps of S7, finishing include: Measure the rolled product to determine the exact location where it needs to be cut, and use the cutting equipment to cut it to the predetermined length; The cut products are straightened by a straightening machine. According to the material and specifications of the products, the pressure, roller distance and straightening speed of the straightening machine are adjusted, and the straightness of the straightened products is checked in real time. Use grinding and polishing methods to remove oxide scale, scratches and minor defects on the product surface; Use non-destructive testing technology to detect defects inside and on the surface of products; Use calipers and micrometers to make detailed measurements of product dimensions and compare the measurement results with design requirements; Take some products for mechanical property testing, analyze the test results, and verify whether the strength and toughness of the products meet the use requirements; Based on the results of the above inspections and tests, the products are graded for quality, qualified products and unqualified products are classified and stored, unqualified products are marked and recorded, and qualified products are packaged.

10. A continuous casting machine low-speed direct rolling process according to claim 1, characterized in that: The specific steps of S8, finished product inspection include: Comprehensively observe the appearance of the finished product to check whether there are cracks, pits, scratches, rust spots or other defects on the surface; Use high-precision measuring tools to accurately measure the key dimensions of length, width, thickness and diameter of the finished product, and compare the measurement results with the dimensional tolerances specified in the product design drawings and relevant standards; Use spectral analysis and chemical analysis to detect the content of various chemical components in the finished product, focusing on whether the content of major alloy elements and harmful impurity elements meets product requirements and relevant standards; Take samples from the finished product for tensile testing to determine the mechanical properties of yield strength, tensile strength and elongation, and conduct hardness testing to evaluate the hardness level of the finished product; For products with special requirements, magnetic properties, electrical properties and thermal conductivity tests are carried out; Observe the microstructure of the finished product through a metallographic microscope to assess whether the microstructure is uniform and dense, and whether there are any abnormal structures; Conduct non-destructive testing review on products that have undergone flaw detection in the finishing stage; According to the above test results, comprehensively determine the quality level of the finished product, record the test data and results in detail, establish a quality file, and provide a basis for quality traceability; For products that fail the inspection, the type and reason of the failure shall be clearly stated.

Citation Information

Cited By

  • Forming process for manufacturing large flat plate type casting blank based on wide and thick continuous casting blank

    CN119952420A

  • Production process of steel for petroleum and natural gas pipe blank

    CN119972850A