Copper metal and processing method and application thereof

By oxidizing, reducing and electrochemical treatment of the copper metal precursor, the porous structure copper metal is formed, which solves the problems of poor safety performance of lithium-ion batteries and printed circuit boards caused by smooth copper metal surface, and achieves high surface roughness and large specific surface area improve the safety performance of lithium-ion batteries and the quality of printed circuit boards.

CN119040868APending Publication Date: 2024-11-29JIANGDONG ELECTRONIC MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149886.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing copper metal has smooth surface and small specific surface area, which is not conducive to inhibiting the growth of lithium dendrites in lithium-ion batteries, affecting safety performance, and poor performance in printed circuit boards.

Method used

By oxidation, reduction and electrochemical treatment of the copper metal precursor, a porous copper metal with high surface roughness and large specific surface area is formed, including electrochemical treatment using a three-electrode system in the alkali liquid, with the number of cycles being 50-1000 times, remove the fibers on the metal surface of the porous fibers and form a micro-nano porous structure.

Benefits of technology

It improves the safety performance of lithium-ion batteries and the quality of printed circuit boards. By inhibiting the growth of lithium dendrites and enhancing the surface roughness and specific surface area, it is suitable for widespread promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040868A_ABST
    Figure CN119040868A_ABST
Patent Text Reader

Abstract

The invention provides copper metal and a processing method and application thereof. The processing method of the copper metal comprises the following steps: carrying out oxidation treatment on a copper metal precursor to obtain a metal oxide precursor; carrying out reduction treatment on the metal oxide precursor to obtain porous fiber copper metal; and performing electrochemical treatment on the porous fiber copper metal to obtain the copper metal. According to the machining method, copper metal with high surface roughness and large specific surface area can be obtained through machining, and the machining method is easy to operate and suitable for wide application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to copper metal and a processing method and application thereof. Background Art

[0002] In recent years, copper metal has been widely used as a current collector in the field of new energy, for example, as a current collector in lithium-ion batteries or printed circuit boards. However, the existing copper metal has a smooth surface and a small specific surface area. When used in lithium-ion batteries, it is not conducive to inhibiting the growth of lithium dendrites in lithium-ion batteries, and thus is not conducive to the safety performance of lithium-ion batteries; and copper metal with a smooth surface and a small specific surface area is not conducive to the performance of printed circuit boards when used in printed circuit boards. Summary of the invention

[0003] The invention provides a copper metal processing method, which can be used to obtain copper metal with high surface roughness and large specific surface area. The processing method is simple to operate and is suitable for wide promotion and application.

[0004] The present invention provides a copper metal obtained by processing using the above-mentioned processing method. The copper metal has high surface roughness and excellent specific surface area. When applied to lithium-ion batteries, it helps to inhibit the growth of lithium dendrites of lithium-ion batteries, thereby improving the safety performance of lithium-ion batteries. When applied to printed circuit boards, it can improve the quality of printed circuit boards.

[0005] The present invention provides an application of copper metal. When the copper metal is applied to a current collector, it helps to inhibit the growth of lithium dendrites of a lithium ion battery, thereby improving the safety performance of the lithium ion battery. When the copper metal is applied to a printed circuit board, it can improve the quality of the printed circuit board.

[0006] The present invention provides a method for processing copper metal, which comprises:

[0007] performing oxidation treatment on a copper metal precursor to obtain a metal oxide precursor;

[0008] Performing a reduction treatment on the metal oxide precursor to obtain a porous fiber copper metal;

[0009] Performing electrochemical treatment on the porous fiber copper metal to obtain the copper metal;

[0010] The electrochemical treatment comprises:

[0011] In an alkaline solution, a three-electrode system was used to perform electrochemical treatment in a potential window of -1V to 1V relative to a Hg / HgO reference electrode at a sweep rate of 1mV / s to 50mV / s.

[0012] The concentration of the alkali solution is 0.1-6 mol / L;

[0013] In the electrochemical treatment, the number of cycles is 50-1000 times.

[0014] The processing method as described above, wherein the oxidation treatment comprises: using an oxidant to oxidize the copper metal precursor;

[0015] The oxidant includes (NH 4 ) 2 S 2 O 8 and NaOH, the oxidant, (NH 4 ) 2 S 2 O 8 The concentration of is 0.5-5 mol / L, the concentration of NaOH is 5-10 mol / L; and / or,

[0016] The reduction treatment includes: using a reducing agent to perform a reduction treatment on the metal oxide precursor;

[0017] The reducing agent comprises dimethylamine borane and NaOH. In the reducing agent, the concentration of dimethylamine borane is 50-100 g / L, and the concentration of NaOH is 10-50 g / L.

[0018] The processing method as described above, wherein the oxidation treatment is performed at a temperature of 25-55° C. and a time of 2 s-2 h; and / or

[0019] During the reduction treatment, the temperature is 25-55° C. and the time is 2s-2h.

[0020] The present invention provides a copper metal, wherein the copper metal is obtained by processing using the processing method as described above.

[0021] The copper metal as described above, wherein the surface of the copper metal has a porous structure with a pore size of 0.6-4 μm.

[0022] The copper metal as described above, wherein the specific surface area of ​​the copper metal is 3-15m 2 / g.

[0023] The present invention provides an application of the copper metal as described above, wherein the copper metal is used for a current collector or a printed circuit board.

[0024] The present invention provides a copper metal processing method, comprising sequentially performing oxidation treatment, reduction treatment and electrochemical treatment on a copper metal precursor to obtain copper metal. The processing method can obtain copper metal with high surface roughness and large specific surface area. The processing method is simple to operate and is suitable for wide promotion and application.

[0025] The present invention provides a copper metal obtained by processing using the above processing method. The copper metal has excellent surface roughness and specific surface area. When applied to lithium-ion batteries, it helps to inhibit the growth of lithium dendrites in lithium-ion batteries, thereby improving the safety performance of lithium-ion batteries. When applied to printed circuit boards, it can improve the quality of printed circuit boards.

[0026] The present invention provides an application of copper metal. When the copper metal is applied to a current collector, it helps to inhibit the growth of lithium dendrites of a lithium ion battery, thereby improving the safety performance of the lithium ion battery. When the copper metal is applied to a printed circuit board, it can improve the quality of the printed circuit board. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 is a SEM image of the copper metal precursor in Example 1 of the present invention;

[0029] Figure 2 is a SEM image of the copper metal obtained in Example 1 of the present invention;

[0030] Figure 3 The cycle performance curves of the Li-Cu half-cells of Experimental Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] A method for processing copper metal, comprising:

[0033] performing oxidation treatment on a copper metal precursor to obtain a metal oxide precursor;

[0034] The metal oxide precursor is subjected to reduction treatment to obtain porous fiber copper metal;

[0035] electrochemically treating the porous fiber copper metal to obtain copper metal;

[0036] Electrochemical treatment includes:

[0037] In an alkaline solution, a three-electrode system was used to perform electrochemical treatment in a potential window of -1V to 1V relative to a Hg / HgO reference electrode at a sweep rate of 1mV / s to 50mV / s.

[0038] The concentration of alkali solution is 0.1-6mol / L;

[0039] In the electrochemical treatment, the number of cycles is 50-1000 times.

[0040] In the present invention, the copper metal precursor may be a copper metal material commonly used in the art, for example, the copper metal precursor may be any one of foamed copper metal, copper-based alloy, and copper metal device.

[0041] Among them, foam copper metal is a porous skeleton structure with a larger specific surface area and higher catalytic properties. It is used in the manufacture of purification, filtration, catalytic brackets, electrodes and other devices in petrochemical, aerospace and environmental protection. Under normal temperature conditions, the foam copper metal is oxidized, reduced and electrochemically treated in sequence to form a series of micro-nanoporous fiber structures on the surface of its porous skeleton to obtain copper metal, further enhancing its application value and scope.

[0042] The copper-based alloy may be at least one of brass, bronze, nickel silver or phosphor copper.

[0043] In some embodiments, the copper metal precursor may be in the form of a metal sheet or a metal film.

[0044] The processing method of the present invention specifically includes: performing an oxidation treatment on a copper metal precursor to oxidize the copper metal precursor into a metal oxide precursor including cuprous oxide and cupric hydroxide; then performing a reduction treatment on the metal oxide precursor to form porous fibers on the surface of the metal oxide precursor, thereby obtaining porous fiber copper metal; and finally performing an electrochemical treatment on the porous fiber copper metal to remove fibers on the surface of the porous fiber copper metal, thereby obtaining copper metal with a porous structure, wherein the obtained porous structure is of micro-nano size.

[0045] The present invention can obtain copper metal with a micro-nano porous structure by sequentially performing oxidation treatment, reduction treatment and electrochemical treatment on a copper metal precursor, and can improve the surface roughness and specific surface area of ​​the copper metal, so that when the copper metal is used in a lithium ion battery, it helps to inhibit the growth of lithium ion battery dendrites, thereby improving the safety performance of the lithium ion battery, and when it is used in a printed circuit board, it can improve the quality of the printed circuit board.

[0046] It is worth mentioning that the processing method of the present invention does not require the introduction and removal of the second phase material, nor does it require acid and alkali corrosion, and has the advantages of simple process, preparation method, and no pollution; and the processing method does not involve special technical processes, has low requirements for equipment, and is low in cost; and the processing method is not affected by the morphology of the copper metal precursor to be processed, and is suitable for processing the surface of complex copper metal precursors.

[0047] In the present invention, the electrochemical treatment comprises:

[0048] In alkaline solution, a three-electrode system was used to perform electrochemical treatment in a potential window of 0 V to 0.5 V relative to a Hg / HgO reference electrode at a scan rate of 50 mV / s.

[0049] The present invention does not particularly limit the alkali solution, and the alkali solution may be an alkali solution commonly used in the art, for example, the alkali solution may be a sodium hydroxide solution and / or a potassium hydroxide solution.

[0050] The present invention uses Hg / HgO as a reference electrode and a porous fiber copper metal to form a battery, and provides and maintains a known and stable potential reference during the test process, which is used to accurately adjust the electrochemical reaction conditions in the electrolyte. Bubbles are generated on the surface of the porous fiber copper metal through the oxygen evolution reaction, and the fiber filament structure on the surface of the porous fiber copper metal is flushed, thereby realizing the in-situ construction of the copper metal micro-nano porous structure. When the electrochemical treatment includes the above-mentioned process, the fibers on the surface of the porous fiber copper metal can be removed more efficiently to obtain copper metal with a micro-nano porous structure, thereby improving the surface roughness and specific surface area of ​​the copper metal.

[0051] Furthermore, when the concentration of the alkali solution is 0.1-6 mol / L, the fibers on the surface of the porous fiber copper metal can be removed more efficiently while saving the alkali solution, thereby obtaining copper metal with a micro-nano porous structure.

[0052] The inventors also found that when the number of cycles in the electrochemical treatment is 50-1000, the fibers on the surface of the porous fiber copper metal can be more fully removed while saving energy, thereby obtaining copper metal with a micro-nano porous structure.

[0053] The present invention does not particularly limit the oxidation treatment and the reduction treatment, and the oxidation treatment and the reduction treatment commonly used in the art may be used.

[0054] In some embodiments of the present invention, the oxidation treatment includes: oxidizing the copper metal precursor using an oxidant;

[0055] Oxidants include (NH 4 ) 2 S 2 O 8and NaOH, oxidizing agent, (NH 4 ) 2 S 2 O 8 The concentration of is 0.5-5mol / L, and the concentration of NaOH is 5-10mol / L.

[0056] When the above-mentioned oxidant is used for oxidation treatment, the oxidation degree of the copper metal precursor can be improved to obtain a metal oxide precursor with a higher surface oxidation degree, which is helpful to obtain micron-level porous and uniformly dispersed copper metal.

[0057] Furthermore, the oxidation treatment may be followed by post-oxidation treatment, wherein the post-oxidation treatment may include: sequentially washing with anhydrous ethanol and deionized water to obtain a metal oxide precursor with less impurity content, thereby helping to improve the purity of the copper metal.

[0058] In some embodiments of the present invention, the reduction treatment includes: performing a reduction treatment on the metal oxide precursor using a reducing agent;

[0059] The reducing agent includes dimethylamine borane and NaOH. In the reducing agent, the concentration of dimethylamine borane is 50-100 g / L, and the concentration of NaOH is 10-50 g / L.

[0060] When the above-mentioned reducing agent is used for reduction treatment, the metal oxide precursor can be more fully reduced to form porous fiber copper metal uniformly dispersed in the porous fibers, which is helpful to obtain micron-level porous and uniformly dispersed copper metal.

[0061] Furthermore, after the reduction treatment, a post-reduction treatment may be included, wherein the post-reduction treatment may include: using anhydrous ethanol and deionized water in sequence for cleaning treatment, so as to obtain a porous fiber copper metal with a low impurity content, thereby helping to improve the purity of the copper metal.

[0062] Further, during the oxidation treatment, the temperature is 25-55°C and the time is 2s-2h; and / or,

[0063] During the reduction treatment, when the temperature is 25-55°C and the time is 2s-2h, the surface area of ​​the copper metal can be further increased.

[0064] A second aspect of the present invention provides copper metal, wherein the copper metal is obtained by processing using the processing method of the first aspect.

[0065] The copper metal of the present invention is obtained by processing through the processing method of the first aspect. The copper metal has high surface roughness and excellent specific surface area. When applied to lithium-ion batteries, it helps to inhibit the growth of lithium dendrites of lithium-ion batteries, thereby improving the safety performance of lithium-ion batteries.

[0066] Furthermore, when the surface of the copper metal has a porous structure with a pore size of 0.6-4 μm, the copper metal has a better specific surface area, which can improve the application effect of the copper metal.

[0067] The inventors also found that when the specific surface area of ​​copper metal is 3-15m 2 / g, when the copper metal is used in lithium-ion batteries, it helps to inhibit the growth of lithium dendrites in lithium-ion batteries, thereby improving the safety performance of lithium-ion batteries.

[0068] A third aspect of the present invention provides a use of the copper metal according to the second aspect, wherein the copper metal is used for a current collector or a printed wiring board.

[0069] Since the current collector of the present invention includes the copper metal, the current collector, when applied to a lithium-ion battery, helps to inhibit the growth of lithium dendrites in the lithium-ion battery, thereby improving the safety performance of the lithium-ion battery. Since the printed circuit board includes the copper metal of the second aspect, the printed circuit board has excellent quality and is suitable for wide promotion and application.

[0070] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0071] Example 1

[0072] The copper metal of this embodiment is prepared by a method comprising the following steps:

[0073] 1) Cut the commercially purchased copper foam into pieces with a surface area of ​​2 cm 2 A copper metal precursor (foam copper precursor) is obtained;

[0074] 2) With water as solvent, the solute (containing only) includes a concentration of 1.0 mol L -1 NH 4 ) 2 S 2 O 8 and 5.0 mol L -1 of NaOH to prepare the oxidant;

[0075] 3) placing the copper metal precursor in step 1) in an oxidant at a temperature of 25° C. for oxidation treatment for 20 minutes, washing with anhydrous ethanol and deionized water in turn, and drying to obtain a metal oxide precursor;

[0076] 4) With water as solvent, the solute (containing only) includes 100.0 g L -1 of dimethylamine borane (DMAB) and 10.0 g L -1 of NaOH to prepare a reducing agent;

[0077] 5) placing the metal oxide precursor in step 3) in a mixed reducing agent at a temperature of 25° C. for reduction treatment for 10 minutes to induce a micro-nano porous fiber structure, and then washing it with anhydrous ethanol and deionized water in turn, and drying it to obtain a porous fiber copper metal;

[0078] 6) using water as solvent and 1 mol / L NaOH as solute to prepare alkali solution (sodium hydroxide solution);

[0079] 7) placing the porous fiber copper metal in step 5) in an alkaline solution, using a three-electrode system, and performing electrochemical treatment (cyclic voltammetry treatment) for 100 cycles at a scan rate of 50 mV / s in a potential window of 0 V to 0.5 V relative to a Hg / HgO reference electrode to obtain copper metal.

[0080] Figure 1 is a SEM image of the copper metal precursor in Example 1 of the present invention; Figure 2 This is a SEM image of the copper metal obtained in Example 1 of the present invention. Figure 1 and Figure 2 It can be seen that by sequentially subjecting the copper metal precursor to oxidation treatment, reduction treatment and electrochemical treatment, a copper metal including a micro-nano porous structure can be formed, wherein the pore size is 0.6-4 μm (the average pore size is 1.5 μm).

[0081] The copper metal precursor, porous fiber copper metal and copper metal with micro-nano porous structure were tested by gas adsorption BET method to obtain the specific surface areas of copper metal precursor, porous fiber copper metal and copper metal with micro-nano porous structure. The specific surface area of ​​copper metal precursor was 0.5m 2 / g, the specific surface area of ​​porous fiber copper metal is 3.5m 2 / g, the specific surface area of ​​copper metal with micro-nano porous structure is 5.6m 2 / g.

[0082] Test Example 1

[0083] The lithium-copper half-cell of this test example was prepared by a method comprising the following steps:

[0084] A lithium sheet is used as the negative electrode, and the copper metal with a micro-nano porous structure in Example 1 is used as the positive electrode to assemble a lithium-copper half-cell, wherein the electrolyte includes LiTFSI, DOL, DME and LiNO 3 , the concentration of LiTFSI in the electrolyte is 1M, LiNO 3 The mass percentage of DME is 5wt%, the volume ratio of DME to DOL is 1:1, and the current density is 1mA cm -2 .

[0085] Test Example 2

[0086] The preparation method of the lithium-copper half-cell of this experimental example is basically the same as that of Experimental Example 1, except that a copper metal precursor is used to replace the copper metal with a micro-nano porous structure.

[0087] Test Example 3

[0088] The preparation method of the lithium-copper half-cell of the experimental example is basically the same as that of the experimental example 1, except that the copper metal with a micro-nano porous structure is replaced by a porous fiber copper metal.

[0089] Performance Testing

[0090] The lithium-copper half-cells of the test examples were respectively subjected to cycle performance tests, and the specific process included:

[0091] Before the battery test, the battery was left for 3 hours to allow the electrolyte in the battery to be fully infiltrated. Then, the battery was tested at a current density of 1 mA cm -2 , the deposition capacity is 1 mAh cm -2 The cycle performance test was carried out under the following conditions. Figure 3 The cycle performance curves of the Li-Cu half-cells of Experimental Examples 1-3 of the present invention (wherein 1 in the figure refers to Experimental Example 1, 2 refers to Experimental Example 2, and 3 refers to Experimental Example 3). Figure 3 It can be seen that the coulombic efficiency of the lithium-copper half-cell of Experimental Example 1 of the present invention remains above 80% after 433 cycles, while the coulombic efficiency of the lithium-copper half-cells of Experimental Examples 2 and 3 drops to 80% after about 295 and 325 cycles, indicating poor stability. This indicates that the copper metal prepared in the embodiment of the present invention can improve the stability of the battery when applied to the battery.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for processing copper metal, It is characterized in that include: performing oxidation treatment on a copper metal precursor to obtain a metal oxide precursor; Performing a reduction treatment on the metal oxide precursor to obtain a porous fiber copper metal; Performing electrochemical treatment on the porous fiber copper metal to obtain the copper metal; The electrochemical treatment comprises: In an alkaline solution, a three-electrode system was used to perform electrochemical treatment in a potential window of -1V to 1V relative to a Hg / HgO reference electrode at a sweep rate of 1mV / s to 50mV / s. The concentration of the alkali solution is 0.1-6 mol / L; In the electrochemical treatment, the number of cycles is 50-1000 times.

2. The processing method according to claim 1, It is characterized in that The oxidation treatment includes: using an oxidant to oxidize the copper metal precursor; The oxidant includes (NH 4 ) 2 S 2 O 8 and NaOH, the oxidant, (NH 4 ) 2 S 2 O 8 The concentration of is 0.5-5mol / L, and the concentration of NaOH is 5-10mol / L.

3. The processing method according to claim 1 or 2, It is characterized in that The reduction treatment includes: using a reducing agent to perform a reduction treatment on the metal oxide precursor; The reducing agent comprises dimethylamine borane and NaOH. In the reducing agent, the concentration of dimethylamine borane is 50-100 g / L, and the concentration of NaOH is 10-50 g / L.

4. The processing method according to claim 1 or 2, It is characterized in that During the oxidation treatment, the temperature is 25-55° C. and the time is 2s-2h.

5. The processing method according to claim 1 or 2, It is characterized in that During the reduction treatment, the temperature is 25-55° C. and the time is 2s-2h.

6. A copper metal, It is characterized in that The product is obtained by processing using the processing method described in any one of claims 1 to 5.

7. The copper metal according to claim 6, It is characterized in that The surface of the copper metal has a porous structure with a pore size of 0.6-4 μm.

8. The copper metal according to claim 6 or 7, It is characterized in that The specific surface area of ​​the copper metal is 3-15m 2 / g.

9. Use of the copper metal according to any one of claims 6 to 8, It is characterized in that The copper metal is used for a current collector or a printed circuit board.