Antibacterial polyamide fiber product and finishing method and application thereof
Through polyamide hydrolase treatment and enzymatic graft polymerization technology, the problem of both antibacterial properties and feel of nylon fiber products is solved, and nylon fiber products with high efficiency antibacterial effects and good feel are achieved, reducing production energy consumption and fiber damage.
Patent Information
- Application Number
- CN202411185474.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
AI Technical Summary
Nylon fiber products are prone to bacteria and mold breeding under suitable conditions, resulting in mold change. The existing antibacterial agents have poor fastness to bond with fibers, insufficient washing resistance, and the finishing process is easy to damage the fibers, making it difficult to take into account both the antibacterial effect and feel.
Nylon fibers are treated with polyamide hydrolase, vinyl groups are introduced, and then enzymatic graft polymerization is carried out in the finishing solution of methacryloyloxyethyltrimethylammonium chloride and horseradish peroxidase to form an antibacterial finishing agent , improve the antibacterial properties of the fiber surface.
It achieves efficient and durable antibacterial effects and has good feel for fiber products, low energy consumption, small fiber damage and high binding fastness, avoiding the problems of lower feel and fiber damage in traditional methods.
Smart Images

Figure BDA0005013368420000081
Abstract
Description
Technical Field
[0001] The invention relates to a nylon fiber product, in particular to an antibacterial nylon fiber product and a finishing method and application thereof. Background Art
[0002] Nylon fiber belongs to polyamide fiber, and its main categories include nylon 6 and nylon 66, which are commonly used synthetic fiber varieties. Compared with polyester fiber, nylon fiber has higher wear resistance, excellent elasticity and strength. Due to the special properties of nylon fiber itself, its fiber products are widely used in many fields. Among them, in clothing, nylon fabrics are often used to make assault jackets, sun-proof clothing, casual clothes, etc.; in home textiles, nylon fiber can be used to make bedding, curtains, carpets, etc.; in the field of sports goods, nylon fiber can be used to make sports socks and basketball jerseys, etc., and is also widely used in the preparation of outdoor equipment (such as tents, etc.).
[0003] Unlike polyester fibers, nylon fibers contain abundant amide bonds and have a moisture regain of about 4.5% under standard atmospheric conditions. Clothing, home textiles and outdoor textiles made of nylon fiber products are prone to become breeding grounds for microorganisms such as bacteria and mold under suitable temperature and humidity conditions, which can cause nylon fiber products to mold and reduce their wearing performance. Therefore, for some high-value-added nylon fiber products, finishing processing is required to improve antibacterial properties.
[0004] The existing antibacterial finishing agents used in fiber products include silver series (silver ions, nanosilver), quaternary ammonium salts, halogenamine compounds, etc. These finishing agents are widely used in the antibacterial finishing of fiber products including cotton, silk and wool fabrics. Although nylon fiber has a certain degree of hydrophilicity, the number of reactive polar groups (such as amino and carboxyl groups) it contains is relatively small. Therefore, when the above antibacterial agents are used in the finishing of nylon fibers, there are problems such as poor bonding strength between the antibacterial agents and the fibers, insufficient washability, etc., and if the process control is not proper during the finishing process, it is easy to cause the fiber strength to be damaged. Resin-type antibacterial agents can form a continuous antibacterial layer on the fiber surface, but their disadvantage is that they can easily cause the feel of the fiber products to decrease. Summary of the invention
[0005] In view of the problem that the antibacterial durability and hand feel of the above-mentioned nylon fiber products cannot be taken into account at the same time, the present invention provides an antibacterial nylon fiber product and its finishing method and application, which has the characteristics of high efficiency and long-lasting antibacterial effect, good hand feel of the fiber product, low energy consumption and little fiber damage.
[0006] In order to achieve the above-mentioned object, the present invention provides a finishing method for antibacterial nylon fiber products on one hand, firstly, the nylon fiber products are treated with polyamide hydrolase to hydrolyze part of the amide bonds in the fiber to produce amino groups, thereby obtaining reactive nylon fiber products; then, 4-vinylbenzylamine is grafted on the surface of the modified nylon fiber products with the help of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to prepare vinyl-containing nylon fiber products; finally, the vinyl-containing nylon fiber products are immersed in a finishing solution composed of methacryloyloxyethyltrimethylammonium chloride and horseradish peroxidase, and the horseradish peroxidase is used to catalyze the graft polymerization of methacryloyloxyethyltrimethylammonium chloride on the surface of the nylon fiber to achieve antibacterial finishing of the nylon fiber products, and the specific process steps are as follows:
[0007] S1. Pretreatment of nylon fiber products: placing the nylon fiber products in a polyamide hydrolase treatment solution for pretreatment, so that the amide bonds in the fibers are hydrolyzed to generate amino groups, thereby obtaining reactive nylon fiber products;
[0008] S2, introducing vinyl groups on the fiber surface: immersing the nylon fiber product treated in step S1 in a treatment solution containing 4-vinylbenzylamine hydrochloride and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to introduce vinyl groups on the fiber surface;
[0009] S3, enzymatic graft polymerization antibacterial agent: using a one-bath two-step method, the nylon fiber product treated in step S2 is immersed in a methacryloyloxyethyltrimethylammonium chloride solution, and then horseradish peroxidase, acetylacetone and hydrogen peroxide are added to catalyze the graft polymerization on the fiber surface to form polymethacryloyloxyethyltrimethylammonium chloride.
[0010] Specifically, in step S1, the concentration of polyamide hydrolase in the treatment solution is 2-4 U / mL, the pH value is 7-8, and the treatment conditions are: temperature 45-50° C., bath ratio 1:(8-10), and treatment time 1.5-3 h.
[0011] Specifically, in step S2, the composition of the treatment liquid is: 4-vinylbenzylamine hydrochloride 5-7.5 g / L, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride 4-8 g / L, N-hydroxysuccinimide 2.5-5 g / L; the treatment conditions are: temperature 25-30°C, pH 4.5-5.5, bath ratio 1:(8-10), and treatment time 4-6 h.
[0012] Preferably, in step S3, the nylon fiber product is immersed in the methacryloyloxyethyltrimethylammonium chloride solution for 30 to 40 minutes.
[0013] Preferably, in step S3, the concentration of methacryloyloxyethyltrimethylammonium chloride in the methacryloyloxyethyltrimethylammonium chloride solution is 15-30 g / L.
[0014] Furthermore, after adding horseradish peroxidase, acetylacetone and hydrogen peroxide, the concentration of horseradish peroxidase is 10-15 U / mL, the concentration of hydrogen peroxide is 0.4-0.8 g / L, and the concentration of acetylacetone is 3-6 g / L; the catalytic treatment conditions are: temperature 35-40° C., pH value 6.5-7.5, bath ratio 1:(8-10), and treatment time 2.5-4 h.
[0015] Preferably, the nylon fiber product comprises yarn, knitted fabric or woven fabric processed with nylon 6 or nylon 66 as fiber raw material.
[0016] Another object of the present invention is to provide a nylon fiber product obtained by finishing the above-mentioned method.
[0017] The third object of the present invention is to provide an application of the above-mentioned nylon fiber product with antibacterial function in the preparation of functional textiles.
[0018] The present invention firstly treats nylon fiber products with the aid of polyamide hydrolase to hydrolyze part of the amide bonds in the fiber to generate amino groups, thereby obtaining reactive nylon fiber products; then, 4-vinylbenzylamine is grafted on the surface of the modified nylon fiber products with the aid of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to prepare vinyl-containing nylon fiber products; finally, the vinyl-containing nylon fiber products are immersed in a finishing solution composed of methacryloyloxyethyltrimethylammonium chloride and horseradish peroxidase, and the horseradish peroxidase catalyzes the grafting polymerization of methacryloyloxyethyltrimethylammonium chloride on the surface of the nylon fiber to achieve antibacterial finishing of the nylon fiber products. Compared with the traditional chemical antibacterial finishing method, the present invention has the following advantages:
[0019] (1) Highly effective and long-lasting antibacterial effect: Vinyl is introduced into the surface of nylon fiber through grafting reaction, and grafting polymerization occurs under the catalysis of biological enzymes. The resulting polymethacryloyloxyethyltrimethylammonium chloride is firmly bonded to the fiber by covalent bonds, which has a high bonding strength. Antibacterial nylon fiber products have a high antibacterial rate and long-lasting antibacterial effect.
[0020] (2) The fiber products have a better feel: Compared with the use of resin-type antibacterial agents with larger molecular weight for antibacterial finishing, the present invention uses horseradish peroxidase-catalyzed graft polymerization to form a polymer network with antibacterial properties on the fiber surface. No macromolecular resins, adhesives or cross-linking agents are added in the antibacterial finishing, and the fiber products have a better feel.
[0021] (3) Low energy consumption and little fiber damage: Conventional nylon fiber products are treated with antibacterial agents applied to the fiber surface by a combination of impregnation and baking, which results in high production energy consumption and the fiber is prone to color change. In contrast, the enzyme-catalyzed antibacterial finishing of nylon fiber products in the present invention is carried out at a lower temperature, with low production energy consumption and little fiber damage. DETAILED DESCRIPTION
[0022] The specific implementation of the present invention is described in detail below in conjunction with the examples. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0023] Embodiment 1:
[0024] (1) Pretreatment of nylon fiber products: Woven fabrics made of nylon 6 were treated with polyamide hydrolase, and then washed and dried; polyamide hydrolase was 2 U / mL, treatment temperature was 45 °C, pH was 7, treatment time was 1.5 h, and bath ratio was 1:10;
[0025] (2) Introducing vinyl groups on the fiber surface: The sample treated in step (1) was immersed in a 4-vinylbenzylamine hydrochloride solution, and vinyl groups were introduced on the fiber surface with the aid of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride; wherein the amount of 4-vinylbenzylamine hydrochloride was 5 g / L, the amount of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride was 4 g / L, and the amount of N-hydroxysuccinimide was 2.5 g / L; the treatment temperature was 25°C, the pH value was 4.5, the treatment time was 4 h, and the bath ratio was 1:10;
[0026] (3) Enzymatic graft polymerization antimicrobial agent: A one-bath two-step method was used to immerse the sample treated in step (2) in a 15 g / L methacryloyloxyethyl trimethyl ammonium chloride solution. After 30 min, horseradish peroxidase, acetylacetone and hydrogen peroxide were added to catalyze the graft polymerization of polymethacryloyloxyethyl trimethyl ammonium chloride on the fiber surface. The fiber was then thoroughly washed with water and dried. The horseradish peroxidase was 10 U / mL, the hydrogen peroxide was 0.4 g / L, and the acetylacetone was 3 g / L. The treatment temperature was 35 °C, the pH value was 6.5, the treatment time was 2.5 h, and the bath ratio was 1:10.
[0027] Embodiment 2:
[0028] (1) Pretreatment of nylon fiber products: nylon knitted fabric made of nylon 66 was treated with polyamide hydrolase, and then washed and dried; wherein the polyamide hydrolase was 4 U / mL, the treatment temperature was 50 °C, the pH was 8, the treatment time was 3 h, and the bath ratio was 1:8;
[0029] (2) Introducing vinyl groups on the fiber surface: The sample treated in step (1) was immersed in a 4-vinylbenzylamine hydrochloride solution, and vinyl groups were introduced on the fiber surface with the aid of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride; wherein the amount of 4-vinylbenzylamine hydrochloride was 7.5 g / L, the amount of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride was 8 g / L, and the amount of N-hydroxysuccinimide was 5 g / L; the treatment temperature was 30°C, the pH value was 5.5, the treatment time was 6 h, and the bath ratio was 1:8;
[0030] (3) Enzymatic graft polymerization antimicrobial agent: A one-bath two-step method was used to immerse the sample treated in step (2) in a 30 g / L methacryloyloxyethyl trimethyl ammonium chloride solution. After 30 min, horseradish peroxidase, acetylacetone and hydrogen peroxide were added to catalyze the graft polymerization of polymethacryloyloxyethyl trimethyl ammonium chloride on the fiber surface. The fiber was then thoroughly washed with water and dried. The horseradish peroxidase was 15 U / mL, the hydrogen peroxide was 0.8 g / L, and the acetylacetone was 6 g / L. The treatment temperature was 40 °C, the pH value was 7.5, the treatment time was 4 h, and the bath ratio was 1:8.
[0031] Comparative Example 1:
[0032] The nylon 6 woven fabric in Example 1 was not subjected to any treatment.
[0033] Comparative Example 2:
[0034] The method in Example 1 is not subjected to step (1) but is subjected to steps (2) and (3) only. Other conditions or descriptions are consistent with those in Example 1.
[0035] Comparative Example 3:
[0036] The method of Example 1 is not subjected to step (2), but only subjected to steps (1) and (3). Other conditions or descriptions are consistent with those of Example 1.
[0037] Comparative Example 4:
[0038] The method of Example 1 was treated by steps (1) to (3), but horseradish peroxidase was not added in step (3). Other conditions or descriptions were consistent with those of Example 1.
[0039] Comparative Example 5:
[0040] The process of Example 1 is carried out through steps (1) to (3), but the process of step (3) adopts a one-bath one-step process, that is, in step (3), the nylon fiber product is immersed in a methacryloyloxyethyltrimethylammonium chloride solution and treated with horseradish peroxidase, and other conditions or descriptions are consistent with those of Example 1.
[0041] Comparative Example 6:
[0042] The sample in Example 1 was treated by steps (1) to (3); then the sample was washed with water at 40° C. for 3 times, each washing time was 15 min, and finally the sample was dried.
[0043] Comparative Example 7:
[0044] The traditional process (impregnation-baking method) was used for antibacterial finishing of nylon woven fabric, wherein the raw materials and specifications of the sample were the same as those of the fabric described in Example 1; the impregnation conditions were: 10 g / L of quaternary ammonium salt modified polyurethane resin type antibacterial agent, and 100% rolling rate at room temperature; and the baking conditions were: the sample was dried at 105°C for 3 min and then baked at 150°C for 1 min.
[0045] Comparative Example 8:
[0046] The nylon 66 knitted fabric in Example 2 without any treatment.
[0047] Comparative Example 9:
[0048] The method of Example 2 is not subjected to step (1), but is subjected to steps (2) and (3). Other conditions or descriptions are consistent with those of Example 2.
[0049] Comparative Example 10:
[0050] The method of Example 2 is not subjected to step (2), but is subjected to steps (1) and (3). Other conditions or descriptions are consistent with those of Example 2.
[0051] Comparative Example 11:
[0052] The method of Example 2 was treated by steps (1) to (3), but horseradish peroxidase was not added in step (3). Other conditions or descriptions were consistent with those of Example 2.
[0053] Comparative Example 12:
[0054] The method of Example 2 is treated by steps (1) to (3), but the one-bath one-step method is adopted in step (3), that is, in step (3), the nylon fiber product is immersed in a methacryloyloxyethyltrimethylammonium chloride solution and horseradish peroxidase is added for treatment, and other conditions or descriptions are consistent with those of Example 2.
[0055] Comparative Example 13:
[0056] The sample in Example 2 was treated by steps (1) to (3); then the sample was washed with water at 40° C. for 3 times, each washing time was 15 min, and finally the sample was dried.
[0057] Comparative Example 14:
[0058] The traditional process (impregnation-baking method) was used for antibacterial finishing of nylon woven fabric, wherein the raw materials and specifications of the sample were the same as those of the nylon knitted fabric described in Example 2; the impregnation conditions were: 10 g / L of quaternary ammonium salt modified polyurethane resin type antibacterial agent, and 100% rolling rate at room temperature; and the baking conditions were: the sample was dried at 105°C for 3 min and then baked at 150°C for 1 min.
[0059] After the above finishing, the properties of the samples in Examples 1 to 2 and Comparative Examples 1 to 14 were measured, specifically including: measuring the warp breaking strength of nylon woven fabrics with reference to GB / T3923.1-2013, measuring the bursting strength of nylon knitted fabrics with reference to GB / T19976-2005; measuring the antibacterial rate of nylon fiber products against Escherichia coli with reference to GB / T 20944.3-2008; measuring the fabric drape coefficient with reference to GB / T23329-2009, and evaluating the feel of the samples. The smaller the drape coefficient, the better the drape and the softer the feel.
[0060] The performance indicators of the samples in Examples 1 to 2 and Comparative Examples 1 to 14 were measured respectively, and the obtained data are listed in Table 1.
[0061] Table 1
[0062]
[0063] From Table 1, we can see that:
[0064] a. The breaking strength and bursting strength of the samples treated with antibacterial finishing by the method described in the present invention (Example 1 and Example 2) are similar to those of the untreated control samples (Comparative Example 1 and Comparative Example 8), indicating that the antibacterial finishing has little effect on the fiber strength and does not cause obvious fiber damage; the antibacterial rate is greater than 99%, indicating that the nylon fiber products treated by the method have good antibacterial properties, that is, polymethacryloyloxyethyltrimethylammonium chloride with strong antibacterial effect is combined on the fiber surface during enzyme-catalyzed graft polymerization; the fabric drape coefficient is similar to that of the untreated control samples (Comparative Example 1 and Comparative Example 8), indicating that the finishing method described in the present invention has little effect on the feel of the fabric.
[0065] b. The strength of the nylon fiber products (Comparative Example 2 and Comparative Example 9) treated only with steps (2) and (3) without step (1) is similar to that of the untreated control samples (Comparative Example 1 and Comparative Example 8); the antibacterial rate of the samples is low, because the fibers are not treated with step (1) and lack amino groups on their surfaces, so that vinyl groups cannot be introduced by grafting 4-vinylbenzylamine in step (2), resulting in the failure of the polymer to form a covalent bond with the fiber surface during enzymatic polymerization, and only a small part of it is adsorbed on the fiber surface by electrostatic force; the fabric drape coefficient is similar to that of the unfinished samples (Comparative Example 1 and Comparative Example 8), and has little effect on the fabric feel.
[0066] c. The strength of the nylon fiber products (Comparative Example 3 and Comparative Example 10) treated only with steps (1) and (3) without step (2) is lower than that of the unfinished control samples (Comparative Example 1 and Comparative Example 8). The reason is related to the hydrolysis of part of the amide bonds of the fiber during the treatment in step (1). The antibacterial rate of the samples is low because the fibers are not treated with step (2), the fiber surface lacks vinyl, and the polymer formed in the enzymatic polymerization does not combine with the fibers. Only a small part is adsorbed on the fiber surface by electrostatic force. The fabric drape coefficient is similar to that of the unfinished samples (Comparative Example 1 and Comparative Example 8), and has little effect on the feel of the fabric.
[0067] d. The nylon fiber products (Comparative Example 4 and Comparative Example 11) treated with steps (1) to (3) but without adding horseradish peroxidase in step (3) had lower strength than the unfinished control samples (Comparative Example 1 and Comparative Example 8). The reason for this is related to the hydrolysis of part of the amide bonds of the fibers in step (1). The antibacterial rate of the samples was low because horseradish peroxidase was not added during the finishing process, and the cationic monomers did not undergo graft polymerization on the fiber surface (no polymer was formed), and only a small part of them was adsorbed on the fiber by electrostatic force. The fabric drape coefficient was lower than that of the unfinished samples (Comparative Example 1 and Comparative Example 8), and the surface fabric felt better.
[0068] e. After the treatment of steps (1) to (3), but the nylon fiber products treated by one-bath one-step method in step (3) (Comparative Example 5, Comparative Example 12) have a strength similar to that of the untreated control samples (Comparative Example 1, Comparative Example 8); the antibacterial rate of the samples is slightly lower than that of the implementation samples (Example 1, Example 2). The reason is that in the one-bath one-step method, the horseradish peroxidase is added too early in the step (3) treatment, resulting in the self-polymerization of part of the cationic monomer (methacryloyloxyethyltrimethylammonium chloride) in the solution before being adsorbed on the fiber surface, affecting the graft polymerization with the nylon fiber, so the antibacterial rate is slightly lower; the fabric drape coefficient is lower than that of the untreated samples (Comparative Example 1, Comparative Example 8), and the surface fabric feels better.
[0069] f. After being treated in steps (1) to (3) and then washed three times at 40°C (15 min each time), the nylon fiber products (Comparative Example 6 and Comparative Example 13) have similar strength, antibacterial rate and drape as the implementation samples (Example 1 and Example 2), indicating that after being treated by the method of the present invention, the polymethacryloyloxyethyltrimethylammonium chloride formed by enzyme-catalyzed graft polymerization on the surface of nylon fiber has a high bonding strength and maintains excellent application performance before washing even after long-term washing.
[0070] g. The nylon fiber products (Comparative Example 7 and Comparative Example 14) treated with antibacterial finishing using the traditional process (impregnation and baking method) are stronger than the untreated control samples (Comparative Example 1 and Comparative Example 8). The reason is related to the formation of an antibacterial resin film layer on the fiber surface. The fiber products have a high antibacterial rate, but a high fabric drape coefficient, indicating that the fabric feel has decreased significantly. The reason is related to the resin film deposited on the fiber surface.
[0071] The preferred implementation modes of the present invention are described in detail above in combination with the embodiments; however, the present invention is not limited to the specific details in the above implementation modes. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical scheme of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0072] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0073] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A finishing method for antibacterial nylon fiber products, characterized in that: The steps include: S1, placing the nylon fiber product in a polyamide hydrolase treatment solution for pretreatment, so that the amide bonds in the fiber are hydrolyzed to produce amino groups, thereby obtaining a reactive nylon fiber product; S2, immersing the nylon fiber product treated in step S1 in a treatment solution containing 4-vinylbenzylamine hydrochloride and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to introduce vinyl groups on the fiber surface; S3, immersing the nylon fiber product treated in step S2 in a methacryloyloxyethyl trimethylammonium chloride solution, and then adding horseradish peroxidase, acetylacetone and hydrogen peroxide to catalyze the graft polymerization on the fiber surface to form polymethacryloyloxyethyl trimethylammonium chloride.
2. The finishing method according to claim 1, characterized in that: In step S1, the concentration of polyamide hydrolase in the treatment solution is 2-4 U / mL, the pH value is 7-8, and the treatment conditions are: temperature 45-50° C., bath ratio 1:(8-10), and treatment time 1.5-3 h.
3. The finishing method according to claim 1, characterized in that: In step S2, the composition of the treatment liquid is: 4-vinylbenzylamine hydrochloride 5-7.5 g / L, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride 4-8 g / L, N-hydroxysuccinimide 2.5-5 g / L; the treatment conditions are: temperature 25-30°C, pH 4.5-5.5, bath ratio 1:(8-10), and treatment time 4-6 h.
4. The finishing method according to claim 1, characterized in that: In step S3, the nylon fiber product is immersed in the methacryloyloxyethyltrimethylammonium chloride solution for 30 to 40 minutes.
5. The finishing method according to claim 1, characterized in that: In step S3, the concentration of methacryloyloxyethyltrimethylammonium chloride in the methacryloyloxyethyltrimethylammonium chloride solution is 15-30 g / L.
6. The finishing method according to claim 5, characterized in that: After adding horseradish peroxidase, acetylacetone and hydrogen peroxide, the concentration of horseradish peroxidase is 10-15 U / mL, the concentration of hydrogen peroxide is 0.4-0.8 g / L, and the concentration of acetylacetone is 3-6 g / L; the catalytic treatment conditions are: temperature 35-40°C, pH value 6.5-7.5, bath ratio 1:(8-10), and treatment time 2.5-4h.
7. The finishing method according to any one of claims 1 to 6, characterized in that: The nylon fiber products include yarns, knitted fabrics or woven fabrics made from nylon 6 or nylon 66 as fiber raw materials.
8. An antibacterial nylon fiber product obtained by finishing with the finishing method according to any one of claims 1 to 7.
9. Use of the antibacterial nylon fiber product according to claim 8 in the preparation of functional textiles.
Citation Information
Cited By
High-strength antibacterial spandex fabric and preparation method thereof
CN122013517A