Method for rapidly and quantitatively testing by-products in crosslinked polyethylene cable insulation

Through the Fourier infrared spectroscopy test method, the problem of difficult measurement of by-product content distribution in crosslinked polyethylene cable insulation is solved, and fast and accurate by-product analysis is achieved, which reduces the testing cost, is suitable for factory on-site use, and provides Data support for the degassing process.

CN119044102APending Publication Date: 2024-11-29XI AN JIAOTONG UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202311502919.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to quickly and accurately test the content distribution of by-products in the insulation of crosslinked polyethylene cables, making it difficult to judge the degassing progress during the degassing process, and the testing method is complex and costly.

Method used

Fourier infrared spectroscopy test method, by impregnating crosslinked polyethylene sheets to control the by-product content, measuring its characteristic peak absorbance, establishing a functional relationship between the mass fraction and relative content of by-products, and taking points along the radial direction of the annular cross-section of the cable , calculate the mass fraction of by-products.

Benefits of technology

It achieves rapid and convenient acquisition of by-product content distribution in cable insulation, reduces testing costs, is suitable for factory on-site use, and provides data support for formulating a degassing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044102A_ABST
    Figure CN119044102A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly and quantitatively testing by-products in crosslinked polyethylene cable insulation, which comprises the following steps: degassing a crosslinked polyethylene sheet, and dipping for different time to obtain a plurality of crosslinked polyethylene samples containing by-products with different mass fractions; carrying out Fourier infrared test on the crosslinked polyethylene sample to obtain the characteristic peak absorbance of the by-product, and calculating the relative content of the by-product according to the characteristic peak absorbance; according to the mass fractions of the by-products in different crosslinked polyethylene samples and the relative contents of the by-products, calculating to obtain a function relationship between the mass fractions and the relative contents of the by-products; cutting a cross-linked polyethylene cable annular section sample; taking points along the radial direction of the annular section sample of the crosslinked polyethylene cable by using a Fourier infrared spectrometer, and measuring to obtain the characteristic peak absorbance of the by-product; according to the characteristic peak absorbance of the by-product, calculating the relative content of the by-product at each measurement point of the annular section sample of the crosslinked polyethylene cable; and calculating the mass fraction of the by-product at each measurement point of the annular cross-section sample of the crosslinked polyethylene cable according to the function relationship.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cross-linked polyethylene cable degassing testing, in particular to a method for rapid quantitative testing of by-products in cross-linked polyethylene cable insulation. Background Art

[0002] Cross-linked polyethylene (XLPE) has good electrical and mechanical properties and is widely used as an insulating material for AC and DC power cables. In the production process of XLPE insulated cables, dicumyl peroxide (DCP) is mainly used as a cross-linking agent to promote the cross-linking of polyethylene to obtain XLPE. Small molecular by-products such as water, methane, α-methylstyrene, acetophenone and cumyl alcohol produced during the cross-linking process will affect the electrical properties and operational safety of XLPE insulated cables. Therefore, it is necessary to degas the cross-linked cable core to remove the small molecular by-products in the XLPE insulation. At present, the determination of the degassing process parameters of the cable core mainly depends on the experience of the manufacturer. However, the size of cables of different voltage levels varies greatly, and it is difficult to determine the appropriate degassing time based on experience alone. Therefore, it is necessary to continuously sample and test the by-product content during the degassing process to determine the degassing effect.

[0003] At present, there are two main methods for testing the by-product content in cable insulation: thermogravimetry and gas chromatography. Thermogravimetry heats the sample to volatilize all the by-products, and the weight difference of the sample before and after heating is calculated as the total content of the residual by-products. Thermogravimetry is relatively simple to operate, but it can only obtain the total content of by-products in the sample, and cannot obtain the accurate content of each by-product. Gas chromatography uses immersion oscillation to make the by-products in the sample enter the solution, and uses a gas chromatograph to measure the by-product content in the solution, and further calculates the by-product content in the sample. Gas chromatography can accurately measure the content of each by-product, but the test operation process is complicated, the test cost is high, and the technical level and analytical ability of the test personnel are also high, which is not conducive to on-site testing in the factory.

[0004] Therefore, it is particularly important to develop a convenient and fast method for testing the by-product content of cable insulation, obtain the content distribution of various by-products in the degassed cable insulation, and accurately evaluate the degassing progress of the cable core.

[0005] The above information disclosed in this Background section is only for enhancement of understanding of the background of the invention and therefore it may contain information that does not form the prior art that is already known to a person of ordinary skill in the art. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for rapid quantitative testing of by-products in cross-linked polyethylene cable insulation, which can quickly obtain the content of various by-products in cable insulation through Fourier transform infrared spectroscopy testing and judge the degassing progress of the cable.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A method for rapid quantitative testing of byproducts in cross-linked polyethylene cable insulation of the present invention comprises:

[0009] Step 1, degassing the cross-linked polyethylene sheet, weighing it with a balance, then using a single by-product to impregnate the completely degassed cross-linked polyethylene sheet, obtaining cross-linked polyethylene samples with different by-product contents by controlling the impregnation time, weighing the impregnated cross-linked polyethylene sample with a balance, and calculating the mass fraction of the by-product in the impregnated cross-linked polyethylene sample;

[0010] Step 2, repeating step 1 multiple times, immersing for different times to obtain multiple cross-linked polyethylene samples containing different mass fractions of by-products;

[0011] Step 3, performing Fourier transform infrared testing on the cross-linked polyethylene sample to obtain the characteristic peak absorbance of the by-product, and calculating the relative content of the by-product according to the characteristic peak absorbance;

[0012] Step 4, calculating the functional relationship between the mass fraction of the by-products and the relative content of the by-products in different cross-linked polyethylene samples;

[0013] Step 5, cutting a cross-linked polyethylene cable annular cross-section sample;

[0014] Step 6, using a Fourier transform infrared spectrometer to measure points along the radial direction of the cross-linked polyethylene cable annular cross-section sample to obtain the characteristic peak absorbance of the by-product;

[0015] Step 7, calculating the relative content of the by-product at each measuring point of the cross-linked polyethylene cable annular cross-section sample according to the characteristic peak absorbance of the by-product;

[0016] Step 8, calculating the mass fraction of the by-products at each measuring point of the cross-linked polyethylene cable annular cross-section sample according to the functional relationship.

[0017] In the method, in step 5, a lathe is used to cut the cross-linked polyethylene cable to be tested to obtain a cross-linked polyethylene cable annular cross-section sample.

[0018] In the method, by-products in the cross-linked polyethylene cable insulation include acetophenone, α-methylstyrene, methane and cumyl alcohol.

[0019] In the method, in step 3, a Fourier transform infrared test is performed on the cross-linked polyethylene sample to obtain a Fourier transform infrared spectrum, and the characteristic peak absorbance of the by-product is obtained based on the Fourier transform infrared spectrum.

[0020] In the method described, steps 1-4 only need to be measured once, and after obtaining the functional relationship between the mass fraction and relative content of the by-products in the cross-linked polyethylene, steps 5-8 only need to be repeated to obtain the mass fraction of the by-products in the cable insulation at different degassing times.

[0021] In the method, cross-linked polyethylene samples with different by-product contents are obtained by increasing the immersion test pieces in equal proportions to control the immersion time.

[0022] In the method, the functional relationship is a linear relationship.

[0023] In the method, the number of points taken in the radial direction is at least 3.

[0024] Beneficial Effects

[0025] The invention quantitatively analyzes by-products at different radial positions of cross-linked polyethylene cable insulation by using a Fourier transform infrared spectrometer, can conveniently and quickly obtain the distribution of by-product content in the tested cable, is convenient for judging the degassing progress of the cable, and is easy and quick to operate by using the Fourier transform infrared spectrometer, has low test cost, and is suitable for long-term use in factories; by studying the changing rules of different by-product contents in the insulation with the degassing time, data support can be provided for formulating the degassing process of the XLPE insulated cable.

[0026] The above description is only an overview of the technical solution of the present invention. In order to make the technical means of the present invention clearer and to enable those skilled in the art to implement it according to the contents of the specification, and to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described below by way of example. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0028] By reading the detailed description of the preferred specific embodiments below, various other advantages and benefits of the present invention will become clear to those of ordinary skill in the art. The drawings in the specification are only for the purpose of illustrating the preferred embodiments and are not considered to be limitations of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can also be obtained based on these drawings without creative work. Moreover, the same reference numerals are used to represent the same components throughout the drawings.

[0029] In the attached picture:

[0030] Figure 1 This is a flow chart of a method for rapid quantitative testing of byproducts in cross-linked polyethylene cable insulation provided by an embodiment of the present disclosure;

[0031] Figure 2 It is a schematic diagram of Fourier infrared spectrum test results of an XLPE sample impregnated with cumyl alcohol provided by an embodiment of the present disclosure;

[0032] Figure 3 A functional relationship diagram of the mass fraction and relative content of cumyl alcohol in XLPE provided in one embodiment of the present disclosure;

[0033] Figure 4 It is a schematic diagram of cable annular cross-section sample sampling and Fourier infrared testing provided by an embodiment of the present disclosure;

[0034] Figure 5 It is a schematic diagram of the mass fraction of cumyl alcohol at each measuring point of the cable sample according to the embodiment of the present disclosure.

[0035] The present invention is further explained below in conjunction with the accompanying drawings and embodiments. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Therefore, the following Figures 1 to 5 The detailed description of the embodiments of the present invention provided in the present invention is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0038] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, it does not require further definition and explanation in subsequent drawings.

[0039] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0040] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0041] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0042] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0043] In order to enable those skilled in the art to better understand the technical solution of the present invention, Figures 1 to 5 The present invention is further described in detail, and the accompanying drawings do not constitute a limitation on the embodiments of the present invention.

[0044] In one embodiment, if Figure 1 As shown, the present disclosure provides a method for rapid quantitative testing of by-products in cross-linked polyethylene cable insulation, comprising the following steps:

[0045] Step 1, degassing the cross-linked polyethylene sheet, weighing it with a balance, then using a single by-product to impregnate the completely degassed cross-linked polyethylene sheet, obtaining cross-linked polyethylene samples with different by-product contents by controlling the impregnation time, weighing the impregnated cross-linked polyethylene sample with a balance, and calculating the mass fraction of the by-product in the impregnated cross-linked polyethylene sample;

[0046] Step 2, repeating step 1 multiple times, immersing for different times to obtain multiple cross-linked polyethylene samples containing different mass fractions of by-products;

[0047] Step 3, performing Fourier transform infrared testing on the cross-linked polyethylene sample to obtain the characteristic peak absorbance of the by-product, and calculating the relative content of the by-product according to the characteristic peak absorbance;

[0048] Step 4, calculating the functional relationship between the mass fraction of the by-products and the relative content of the by-products in different cross-linked polyethylene samples;

[0049] Step 5, cutting a cross-linked polyethylene cable annular cross-section sample;

[0050] Step 6, using a Fourier transform infrared spectrometer to measure points along the radial direction of the cross-linked polyethylene cable annular cross-section sample to obtain the characteristic peak absorbance of the by-product;

[0051] Step 7, calculating the relative content of the by-product at each measuring point of the cross-linked polyethylene cable annular cross-section sample according to the characteristic peak absorbance of the by-product;

[0052] Step 8, calculating the mass fraction of the by-products at each measuring point of the cross-linked polyethylene cable annular cross-section sample according to the functional relationship.

[0053] In a preferred embodiment of the method, in step 5, a lathe is used to cut the cross-linked polyethylene cable to be tested to obtain a cross-linked polyethylene cable annular cross-section sample.

[0054] In a preferred embodiment of the method, the by-products in the cross-linked polyethylene cable insulation include acetophenone, α-methylstyrene, methane, cumyl alcohol and water.

[0055] In a preferred embodiment of the method, the content of by-product cumyl alcohol in cross-linked polyethylene cable insulation is determined according to 3370 cm -1 Absorbance of characteristic peak of cumyl alcohol A 3370 and 2020cm -1 Absorbance of characteristic peak of methylene at A 2020 The relative content of cumyl alcohol is calculated by the ratio of C = A 3370 / A 2020 .

[0056] In a preferred embodiment of the method, in step 3, a Fourier transform infrared test is performed on the cross-linked polyethylene sample to obtain a Fourier transform infrared spectrum, and the characteristic peak absorbance of the by-product is obtained based on the Fourier transform infrared spectrum.

[0057] In a preferred embodiment of the method, steps 1-4 only need to be measured once, and after obtaining the functional relationship between the mass fraction and relative content of the by-products in the cross-linked polyethylene, steps 5-8 only need to be repeated to obtain the mass fraction of the by-products in the cable insulation at different degassing times.

[0058] In a preferred embodiment of the method, cross-linked polyethylene samples with different by-product contents are obtained by increasing the immersion test pieces in equal proportions to control the immersion time.

[0059] In a preferred embodiment of the method, the functional relationship is a linear relationship.

[0060] In a preferred embodiment of the method, the number of points in the radial direction is at least 3.

[0061] In one embodiment, the method includes measuring the weight change before and after the XLPE sample is impregnated with the by-product; measuring the Fourier infrared spectrogram after the XLPE sample is impregnated with the by-product; fitting to obtain the functional relationship between the relative content and mass fraction of the by-product in the XLPE; cutting a ring-shaped cross-section sample from the middle of the measured cable segment; using a Fourier infrared spectrometer to measure points along the radial direction of the ring-shaped sample; calculating the relative content of the by-product at each measurement point according to the characteristic peak height and converting it into a mass fraction to obtain the distribution of the by-product content in the radial direction of the cable insulation. Among them, by measuring the weight change before and after the XLPE sample is impregnated with the by-product, and measuring the Fourier infrared spectrogram after the XLPE sample is impregnated with the by-product, the relative content and mass fraction of the by-product in multiple groups of XLPE are obtained, and the functional relationship between the two can be fitted. By cutting the cable ring-shaped cross-section sample and taking points in the radial direction of the ring-shaped sample for Fourier infrared spectroscopy testing, the relative content distribution of the by-product in the radial direction of the cable insulation can be quickly obtained. According to the functional relationship and the relative content distribution of the by-product in the radial direction of the cable insulation, the distribution of the by-product mass fraction in the radial direction of the cable insulation can be calculated.

[0062] In one embodiment, if Figure 1 As shown, a rapid quantitative method for by-products in cross-linked polyethylene cable insulation comprises the following steps:

[0063] (1) The XLPE sheet is completely degassed and its weight m1 is weighed on a balance. Then, the XLPE sheet is immersed in cumyl alcohol for a period of time. The weight of the immersed XLPE sample is weighed on a balance m2, and the mass fraction of cumyl alcohol in the XLPE sample is calculated to be W = (m2-m1) / m1;

[0064] (2) repeating step (1) and immersing for different times to obtain a plurality of XLPE samples containing different mass fractions of cumyl alcohol;

[0065] (3) The XLPE sample was subjected to Fourier infrared testing, and the test results were as follows: Figure 2 As shown, according to 3370cm -1 Absorbance of characteristic peak of cumyl alcohol A 3370 and 2020cm -1 Absorbance of characteristic peak of methylene at A 2020 The relative content of cumyl alcohol is calculated by the ratio of C = A 3370 / A 2020 ;

[0066] (4) The functional relationship between the mass fraction W and relative content C of cumyl alcohol in different XLPE samples was obtained by fitting, as shown in Figure 2. Figure 3 As shown;

[0067] (5) Use a lathe to cut the cable ring section specimen, such as Figure 4 As shown;

[0068] (6) Use a Fourier transform infrared spectrometer to measure points along the radial direction of the cable ring cross-section sample, such as Figure 4 As shown;

[0069] (7) According to the height A of the characteristic peaks of cumyl alcohol and methylene in the measurement results at each point 3370 and A 2020 Calculate the relative content C of cumyl alcohol at each measuring point of the cable sample;

[0070] (8) Based on the functional relationship between the relative content and mass fraction of the by-products, the mass fraction W of cumyl alcohol at each measuring point of the cable sample at different degassing times was calculated. The results are shown in Figure 5 shown.

[0071] In this embodiment, according to the Lambert-Beer law, cumyl alcohol has a -1 The relationship between the absorption intensity of the light and the concentration of cumyl alcohol and the thickness of the sample is:

[0072] A 3370 =k 枯基醇 M 枯基醇 d (1)

[0073] Where: A 3370 —The absorbance of the characteristic functional group hydroxyl (-OH) of cumyl alcohol in XLPE samples;

[0074] K 枯基醇 — Cumyl alcohol at 3370 cm -1 Molar absorption coefficient at-1 cm -1 ;

[0075] M 枯基醇 —Molar concentration of cumyl alcohol in XLPE, mol·L -1 ;

[0076] d—thickness of the XLPE sample being tested, cm.

[0077] From formula (1), we can know that the XLPE sample has a -1 The absorbance at is not only affected by the molar absorption coefficient and molar concentration of cumyl alcohol, but also by the thickness of the sample. In order to eliminate the influence of sample thickness differences on the accuracy of the measurement results, the absorption peak with a fixed concentration in XLPE is usually selected as the reference internal standard peak, and the ratio of the characteristic peak absorption intensity of a certain cross-linked byproduct to the internal standard peak intensity is used as the relative content of the substance. Since the characteristic absorption peak of the methylene (-CH2-) group of the XLPE skeleton group is only related to the sample thickness, the bending vibration peak of the methylene is selected as the reference peak, and its wave number is 2020cm -1 .

[0078] The relative content of cumyl alcohol in XLPE is C 枯基醇 Equal to the absorbance of cumyl alcohol A 3370 Absorbance of characteristic peak of methylene 2020 Ratio of:

[0079]

[0080] Where: A 2020 —The absorbance of methylene in XLPE sample;

[0081] k 亚甲基 —Methylene in 2020cm -1 Molar absorption coefficient at -1 cm -1 ;

[0082] M 亚甲基 —Molar concentration of methylene in XLPE, mol·L -1 ;

[0083] B—cumyl alcohol at 3370 cm -1 Absorption coefficient k 枯基醇 With methylene at 2020cm -1 Absorption coefficient k 亚甲基 and its concentration M 亚甲基 The ratio of , a constant.

[0084] From formula (2), we can know that the relative content of cumyl alcohol in XLPE sample is 枯基醇 Its molar concentration M枯基醇 Directly proportional.

[0085] Cumyl alcohol mass fraction in XLPE W 枯基醇 With molar concentration M 枯基醇 The relationship is:

[0086]

[0087] From formula (3), we can know that the mass fraction of cumyl alcohol in XLPE is W 枯基醇 Its molar concentration M 枯基醇 The mass fraction of cumyl alcohol in XLPE is W 枯基醇 The relative content of C 枯基醇 Therefore, in step (4), a linear function can be used to fit the functional relationship between the two, and applied to step (8) to obtain the mass fraction of cumyl alcohol at each measuring point.

[0088] Although the embodiments of the present invention are described above in conjunction with the accompanying drawings, the present invention is not limited to the above specific embodiments and application fields, and the above specific embodiments are only illustrative and instructive, rather than restrictive. A person of ordinary skill in the art can also make many forms under the guidance of this specification and without departing from the scope of protection of the claims of the present invention, all of which belong to the protection of the present invention.

Claims

1. A rapid quantitative test method for by-products in cross-linked polyethylene cable insulation, characterized in that: It includes the following steps: Step 1, calculating the mass fraction of by-products in the impregnated cross-linked polyethylene sample; Step 2, repeating step 1 multiple times, immersing for different times to obtain multiple cross-linked polyethylene samples containing different mass fractions of by-products; Step 3, calculating the relative content of by-products according to the characteristic peak absorbance; Step 4, calculating the functional relationship between the by-product mass fraction and the by-product relative content in different cross-linked polyethylene samples.

2. The method according to claim 1, characterized in that Preferably, a lathe is used to cut the cross-linked polyethylene cable to be tested to obtain a cross-linked polyethylene cable annular cross-section sample.

3. The method according to claim 1, characterized in that By-products in cross-linked polyethylene cable insulation include acetophenone, α-methylstyrene, methane, cumyl alcohol and water.

4. The method according to claim 1, characterized in that In step 3, a Fourier transform infrared (FTIR) test is performed on the cross-linked polyethylene sample to obtain a FTIR spectrum, and the characteristic peak absorbance of the by-product is obtained based on the FTIR spectrum.

5. The method according to claim 1, characterized in that Steps 1-4 only need to be measured once.

6. The method according to claim 1, characterized in that Cross-linked polyethylene samples with different by-product contents were obtained by increasing the impregnation specimens in equal proportions and controlling the impregnation time.

7. The method according to claim 1, characterized in that The functional relationship is a linear relationship.

Citation Information

Cited By

  • Detection method of cable degassing by-products

    CN119310030A

  • Submarine cable factory joint degassing byproduct detection method and device based on machine learning

    CN121231270A