Positive electrode material, positive plate and battery

By forming a spinel structure cladding layer and a fast ion conductor cladding layer on the surface of the lithium-rich manganese-based positive electrode material, the structural instability and irreversible phase change of the material are solved, and the cycle performance and stability of the battery are improved. , improves the battery's first-effect and rate performance.

CN119050334APending Publication Date: 2024-11-29ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411433236.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Lithium-rich manganese-based positive electrode materials have problems such as instability in structure, low first efficiency, poor magnification, fast attenuation of cyclic process voltage and capacity, mainly due to the escape of lattice oxygen and irreversible phase change.

Method used

Using a first cladding layer including a spinel structure and a second cladding layer of an oxide material or a carbon material containing a fast ion conductor, prevents lattice oxygen from escaping and irreversible phase change, improves the transmission speed of lithium ions, and The contact between the lithium-rich manganese-based material and the electrolyte is reduced by the second cladding layer, thereby enhancing surface stability.

Benefits of technology

It improves the structural stability and cyclic performance of the positive electrode material, improves the first-effect and rate performance, reduces the cyclic voltage drop of the battery, and extends the cyclic stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050334A_ABST
    Figure CN119050334A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a positive electrode material and a positive plate battery comprising the positive electrode material. The positive electrode material comprises a lithium-rich manganese-based material, a first material and a second material, the first material comprises a spinel structure, and the second material comprises an oxide material containing a fast ion conductor and / or a carbon material containing a fast ion conductor; the first material forms a first coating layer on the surface of the lithium-rich manganese-based material, the second material coats the surface of the first coating layer to form a second coating layer, and in the second coating layer, a fast ion conductor is located inside and / or on the surface of the oxide material and / or the carbon material. The positive electrode material disclosed by the invention is stable in structure, relatively high in first efficiency and relatively good in rate capability, the cycle stability of the battery is improved, and the cycle voltage drop of the battery is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a positive electrode material and a positive electrode sheet battery comprising the positive electrode material. Background Art

[0002] The lithium-rich manganese-based material has a specific capacity of more than 250mAh / g, which is much higher than the commercialized positive electrode materials such as lithium cobalt oxide, lithium iron phosphate, and nickel-cobalt-manganese ternary. On the other hand, the lithium-rich manganese-based material has a lower cost than lithium cobalt oxide and nickel-cobalt-manganese ternary. Therefore, the lithium-rich manganese-based material is considered to be the most promising next-generation lithium-ion battery positive electrode material. However, the lithium-rich manganese-based material has a series of problems such as unstable structure, low initial efficiency, poor rate, and fast voltage and capacity decay during the cycle process, which seriously restricts the commercialization process of lithium-rich manganese-based positive electrode materials. Summary of the invention

[0003] Research has found that the main reason for the above-mentioned problems of lithium-rich manganese-based materials is the escape of lattice oxygen and irreversible phase change in the lithium-rich manganese-based positive electrode materials during the cycle process.

[0004] In order to overcome the problems of lattice oxygen escape and irreversible phase change in lithium-rich manganese-based positive electrode materials, the present invention provides a positive electrode material, the spinel structure in the positive electrode material can effectively prevent the escape of lattice oxygen and inhibit irreversible phase change of the lithium-rich manganese-based material, thereby improving the cycle performance of the lithium-rich manganese-based material and improving the first efficiency and rate of the battery; the fast ion conductor contained in the positive electrode material can effectively increase the transmission speed of lithium ions, and at the same time, the coating layer on the surface of the positive electrode material can reduce or even block the direct contact between the lithium-rich manganese-based material and the electrolyte, avoid the dissolution of transition metals in the lithium-rich manganese-based material, improve the surface stability of the lithium-rich manganese-based material, improve the capacity retention rate during the battery cycle and reduce the voltage drop.

[0005] A first aspect of the present invention provides a positive electrode material, wherein the positive electrode material includes a lithium-rich manganese-based material, a first material and a second material, the first material includes a spinel structure, and the second material includes an oxide material containing a fast ion conductor and / or a carbon material containing a fast ion conductor; the first material forms a first coating layer on the surface of the lithium-rich manganese-based material, and the second material is coated on the surface of the first coating layer to form a second coating layer, in which the fast ion conductor is located inside and / or on the surface of the oxide material and / or the carbon material.

[0006] A second aspect of the present invention provides a positive electrode sheet, which includes the positive electrode material described in the first aspect of the present invention.

[0007] A third aspect of the present invention provides a battery, comprising the positive electrode sheet according to the second aspect of the present invention.

[0008] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:

[0009] The positive electrode material of the present invention forms a first coating layer including a spinel structure by in-situ coating on the surface of a lithium-rich manganese-based material, and a second coating layer formed on the surface of the first coating layer by a second material including an oxide material containing a fast ion conductor and / or a carbon material, thereby improving the structural stability of the positive electrode material and solving the problem that the lithium-rich manganese-based material is prone to lattice oxygen escape and irreversible phase change. Firstly, since the first coating layer includes a spinel structure, the presence of the spinel structure can effectively inhibit the lattice oxygen escape and irreversible phase change on the surface of the lithium-rich manganese-based material, thereby improving the structural stability of the positive electrode material and at the same time improving the transmission rate of lithium ions, thereby improving the positive electrode material. The first efficiency and rate performance of the positive electrode material are improved, while the cycle stability of the battery and the stability of the cycle voltage drop are improved. Secondly, a second coating layer is coated on the surface of the first coating layer and is formed by a second material including an oxide material and / or a carbon material containing a fast ion conductor, wherein the oxide material and / or the carbon material contains a fast ion conductor, which can further increase the lithium ion transmission speed, improve the first efficiency and rate performance of the positive electrode material, and at the same time, the second coating layer reduces or even avoids the direct contact between the positive electrode material and the electrolyte, reduces the side reaction between the positive electrode material and the electrolyte, and avoids the dissolution of transition metals in the lithium-rich material, thereby improving the battery cycle stability and reducing the battery cycle voltage drop.

[0010] Other features and advantages of the present invention will be described in detail in the following detailed description.

[0011] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The figure shows one of the structural schematic diagrams of the positive electrode material in one embodiment of the present invention.

[0013] Figure 2 The figure shows the second structural schematic diagram of the positive electrode material in one embodiment of the present invention.

[0014] Figure 3 Shown is the XRD spectrum of the positive electrode material in one embodiment of the present invention.

[0015] Figure 4 Shown Figure 3 A is an enlarged view of the middle image.

[0016] Figure 5 Shown is a schematic structural diagram of the oxide material containing a fast ion conductor in the present invention.

[0017] Figure 6 Shown is a schematic structural diagram of the carbon material containing a fast ion conductor in the present invention.

[0018] Figure 7 Shown is a SEM image of an uncoated lithium-rich manganese-based material.

[0019] Figure 8 Shown is a SEM image of the positive electrode material in one embodiment of the present invention. DETAILED DESCRIPTION

[0020] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not used to limit the present invention. In this article, unless otherwise specified, the data range includes the endpoints.

[0021] It should be noted that the numerical expressions such as "first" and "second" in the present disclosure are only used to distinguish different substances or usage methods, and do not represent the difference in order.

[0022] A first aspect of the present invention provides a positive electrode material, wherein the positive electrode material includes a lithium-rich manganese-based material, a first material and a second material, the first material includes a spinel structure, and the second material includes an oxide material containing a fast ion conductor and / or a carbon material containing a fast ion conductor; the first material forms a first coating layer on the surface of the lithium-rich manganese-based material, and the second material is coated on the surface of the first coating layer to form a second coating layer, in which the fast ion conductor is located inside and / or on the surface of the oxide material and / or the carbon material.

[0023] like Figure 1 , Figure 2 , Figure 5 and Figure 6 As shown, the positive electrode material includes a lithium-rich manganese-based material 1, a first material and a second material, the first material forms a first coating layer 2 on the surface of the lithium-rich manganese-based material 1, the second material is coated on the surface of the first coating layer 2 to form a second coating layer 3, in the second coating layer 3, the fast ion conductor 31 is located inside and / or on the surface of the oxide material 32 and / or the carbon material 33, together forming a coating layer 3, wherein the second coating layer 3 formed by the second material can be non-continuously coated on the surface of the first coating layer 2, for example, island-shaped coated on the surface of the first coating layer 2 (such as Figure 1 As shown), it can also be continuously coated on the surface of the first coating layer 2 (as shown Figure 2As shown in FIG. 1 ), the fast ion conductor 31 is located inside and / or on the surface of the oxide material 32 and / or the carbon material 33. Figure 5 As shown, the fast ion conductor 31 is located inside and on the surface of the oxide material 32; Figure 6 As shown, the fast ion conductor 31 is located inside and on the surface of the carbon material 33 .

[0024] The first coating layer includes a spinel structure, which can inhibit the escape of lattice oxygen of lithium-rich manganese-based materials and inhibit irreversible phase changes, and can also improve the transmission rate of lithium ions. Therefore, while protecting the lithium-rich manganese-based materials, the first coating layer can also improve the first efficiency and rate performance of the positive electrode material, improve the cycle stability of the battery and reduce the voltage drop of the cycle voltage of the battery. In order to further improve the structural stability of the positive electrode material, reduce or even avoid the side reaction between the lithium-rich manganese-based material and the electrolyte, a second coating layer including a second material is formed on the surface of the first coating layer. It can be understood that whether it is an island-shaped coated second coating layer or a continuously coated second coating layer, the second coating layer can achieve the effect of isolating the lithium-rich manganese-based material from the electrolyte, reduce or even avoid direct contact between the lithium-rich manganese-based material and the electrolyte, reduce the side reaction between the lithium-rich manganese-based material and the electrolyte, avoid the dissolution of transition metals in the positive electrode material, and further improve the structural stability of the positive electrode material. At the same time, by loading the fast ion conductor in the oxide material and the carbon material, The fast ion conductor can be uniformly dispersed in the second coating layer along with the second material, and the fast ion conductor can improve the lithium ion transfer rate of the positive electrode material. The fast ion conductor uniformly dispersed in the second coating layer can further improve the lithium ion transfer rate of the positive electrode material, thereby further improving the first efficiency and rate performance of the positive electrode material, and the carbon material can improve the electronic conductivity of the positive electrode material. Further, the second coating layer can also simultaneously improve the ionic conductivity and electronic conductivity of the positive electrode material. No matter the second coating layer is an island coating or a continuous coating structure, it is tightly combined with the first coating layer and is not easy to fall off, which can further improve the structural stability of the positive electrode material.

[0025] In the present invention, by using spinel and oxide materials and carbon materials containing fast ion conductors to coat lithium-rich manganese-based materials to form a tightly bonded coating layer, compared with the prior art, the positive electrode can achieve higher stability and higher first efficiency and rate performance, thereby improving the cycle stability of the battery and reducing the voltage drop of the cycle voltage of the battery. In order to further improve the effect, one or more of the technical features can be further optimized.

[0026] like Figure 1 and Figure 2 As shown, the first interface 12 between the first coating layer and the lithium-rich manganese-based material is an interface structure in which the first material and the lithium-rich manganese-based material are interwoven and mixed.

[0027] like Figure 1 and Figure 2 As shown, the second interface 23 between the second coating layer and the first coating layer is an interface structure in which the second material and the first material are interwoven and mixed.

[0028] In the present invention, the spinel structure is a manganese-based material having a spinel structure, and its chemical formula can be expressed as LiNi a Co b Mn c O4, where a+b+c=2. a, b, c can be decimals or integers.

[0029] In one example, the second material includes an oxide material containing a fast ion conductor, and the second material is coated on the surface of the first coating layer to form a continuous second coating layer.

[0030] In one example, the second material includes a carbon material containing a fast ion conductor, and the second material is coated on the surface of the first coating layer to form an island-shaped second coating layer.

[0031] In one example, the first coating layer is a coating layer formed in situ on the surface of the lithium-rich manganese-based material. The coating layer formed in situ on the surface of the lithium-rich manganese-based material can make the coating layer more tightly combined with the lithium-rich manganese-based material, and the coating layer formed in situ is more uniform and dense. The structural stability, especially the mechanical properties, of the positive electrode material in situ coated on the surface of the lithium-rich manganese-based material are further improved, and the uniform and dense coating layer further improves the rate performance of the positive electrode material. In the present invention, the in situ refers to a coating layer formed by a chemical reaction on the surface of the lithium-rich manganese-based material, which is referred to as a coating layer formed in situ. The first coating layer of the present invention is a coating layer formed by a chemical reaction on the surface of the lithium-rich manganese-based material during the preparation process of the lithium-rich manganese-based material.

[0032] In one example, the oxide material has a porous structure, and the fast ion conductor is embedded in the pores or on the surface of the oxide material. Embedding the fast ion conductor in the pores of the oxide material can make the fast ion conductor more uniformly dispersed in the second coating layer, so that the fast ion conductor can form an ion transmission network in the second coating layer, further improving the lithium ion transmission rate of the positive electrode material, thereby further improving the first efficiency and rate performance of the positive electrode material.

[0033] like Figure 5 As shown, the oxide material 32 has a porous structure, both ends of the pores in the oxide material are connected to the surface of the oxide material and / or one end is connected to the surface of the oxide material, and the fast ion conductor 31 is embedded in the pores and / or on the surface of the oxide material 32.

[0034] In one example, based on the total weight of the oxide material containing the fast ion conductor, the weight content of the fast ion conductor is 10%-20% (for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%). Controlling the content of the fast ion conductor within the above range can enable the positive electrode material to have higher ion conductivity and higher capacity. When the content of the fast ion conductor is lower than 10%, the content of the fast ion conductor in the positive electrode material is too low, and the improvement of the ion conductivity of the positive electrode material is not obvious; when the content of the fast ion conductor is higher than 20%, the thickness of the second coating layer increases, causing the thickness of the coating layer of the positive electrode material to be too large, thereby reducing the capacity of the positive electrode material.

[0035] In one example, based on the total weight of the oxide material containing a fast ion conductor, the weight content of the fast ion conductor is 13%-17%.

[0036] In one example, the carbon material has a porous structure, and the fast ion conductor is embedded in the pores of the carbon material. Embedding the fast ion conductor in the pores of the carbon material can make the fast ion conductor more uniformly dispersed in the second coating layer, so that the fast ion conductor can form an ion and electron transport network in the second coating layer, further improving the lithium ion transport rate and electronic conductivity of the positive electrode material, thereby further improving the first efficiency and rate performance of the positive electrode material.

[0037] like Figure 6 As shown, the carbon material 33 has a porous structure, both ends of the pores in the carbon material are connected to the surface of the oxide material and / or one end is connected to the surface of the oxide material, and the fast ion conductor 31 is embedded in the pores and / or on the surface of the carbon material 32.

[0038] In one example, based on the total weight of the carbon material containing the fast ion conductor, the weight content of the fast ion conductor is 10%-20% (for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%). Controlling the content of the fast ion conductor within the above range can enable the positive electrode material to have higher ion conductivity and higher electronic conductivity while having higher capacity. When the content of the fast ion conductor is lower than 10%, the content of the fast ion conductor in the positive electrode material is too low, and the improvement of the ion conductivity of the positive electrode material is not obvious; when the content of the fast ion conductor is higher than 20%, the thickness of the first coating layer and the second coating layer increases, resulting in the thickness of the coating layer of the positive electrode material being too large, thereby reducing the capacity of the positive electrode material.

[0039] In one example, based on the total weight of the carbon material containing a fast ion conductor, the weight content of the fast ion conductor is 13%-17%.

[0040] In one example, the fast ion conductor includes one or more of lithium phosphotungstate, lithium phosphate, and lithium phosphomolybdate.

[0041] In one example, the oxide material includes one or more of zirconium dioxide, titanium dioxide, aluminum oxide, and silicon dioxide.

[0042] In one example, the carbon material includes one or more of activated carbon, graphite and carbon nanotubes.

[0043] In one example, the lithium-rich manganese-based material includes a chemical formula of xLi2MnO3·(1-x)LiNi a Co b Mn c Particles of O2, wherein 0<x<1 (for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 0.95), 0≤a≤1 (for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1), 0≤b≤1 (for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1), 0≤c≤1 (for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1), and a+b+c=1.

[0044] When a=0, it means that the lithium-rich manganese-based material does not include Ni element.

[0045] When b=0, it means that the lithium-rich manganese-based material does not include the Co element.

[0046] When c=0, it means that the lithium-rich manganese-based material does not include the Mn element.

[0047] It is understandable that a, b, and c cannot be 0 at the same time. Moreover, the values ​​of a, b, and c can satisfy the principle that the algebraic sum of the positive and negative valences of the elements in the chemical formula is zero.

[0048] In one example, the thickness of the second coating layer is greater than or equal to the thickness of the first coating layer. When the thickness of the second coating layer is less than the thickness of the first coating layer, the thickness of the first coating layer including the spinel structure is too thick, resulting in a decrease in the capacity of the positive electrode material, and also hindering the transmission of ions and the battery, resulting in a decrease in the first efficiency and rate performance of the positive electrode material.

[0049] In one example, the thickness of the second coating layer is greater than the thickness of the first coating layer.

[0050] In one example, the ratio of the thickness of the first coating layer to the thickness of the second coating layer is 1:(1-5) (for example, 1:1, 1:2, 1:3, 1:4 or 1:5). The thickness of the first coating layer has a certain correlation with the thickness of the second coating layer. When the ratio of the thickness of the first coating layer to the thickness of the second coating layer is lower than 1:5, the thickness of the first coating layer is too thin, and the improvement of the first efficiency and rate performance of the positive electrode material is not obvious, and the protective effect on the positive electrode material is weak, so that the improvement of the cycle stability of the battery and the voltage drop of the cycle voltage is not obvious; when the ratio of the thickness of the first coating layer to the thickness of the second coating layer is higher than 1:1, the thickness of the first coating layer is too thick, which will affect the transmission of ions and electrons in the positive electrode material, resulting in a decrease in the first efficiency and rate performance of the positive electrode material, and at the same time, the capacity of the positive electrode material will be reduced. When the ratio of the thickness of the first coating layer to the thickness of the second coating layer is within the above range, the positive electrode material can have a higher capacity while significantly improving the first efficiency and rate performance.

[0051] In one example, the thickness of the first coating layer is 2nm-8nm (for example, 2nm, 2.5nm, 3nm, 3.5nm, 4nm, 4.5nm, 5nm, 5.5nm, 6nm, 6.5nm, 7nm, 7.5nm or 8nm). The thickness of the first coating layer can be uniform or non-uniform. When the thickness of the first coating layer is non-uniform, the thickness of the first coating layer is the average value of the thickness at the thinnest part and the thickness at the thickest part of the first coating layer. The thickness of the first coating layer can be obtained by testing using conventional technical means in the art, such as SEM and TEM.

[0052] In an example where the second coating layer is a continuous coating, the thickness of the second coating layer is 2nm-10nm (for example, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm or 10nm). The thickness of the second coating layer can be uniform or non-uniform. When the thickness of the second coating layer is non-uniform, the thickness of the second coating layer is the average value of the thickness at the thinnest part and the thickness at the thickest part of the second coating layer. The thickness of the second coating layer can be measured by conventional technical means in the art, such as SEM and TEM.

[0053] According to a specific embodiment, the ratio of the thickness of the first coating layer to the thickness of the second coating layer is 1: (1-5), and based on the total weight of the oxide material containing the fast ion conductor, the weight content of the fast ion conductor is 10%-20%, and the thickness of the first coating layer is 2nm-8nm, and the thickness of the second coating layer is 2nm-10nm. The content of the fast ion conductor in the oxide material will affect the thickness of the first coating layer. At the same time, controlling the content of the fast ion conductor in the oxide material, the thickness of the first coating layer and the thickness of the second coating layer and the ratio of the thicknesses of the two can improve the comprehensive performance of the positive electrode material, so that the comprehensive performance of the positive electrode material is better, for example, higher first efficiency, better rate performance and higher capacity.

[0054] In one example, the first coating layer completely covers the lithium-rich manganese-based material.

[0055] In one example, the second coating layer covers a portion or the entire surface of the first coating layer.

[0056] In one example, the second coating layer covers the entire surface of the first coating layer.

[0057] In one example, the first coating layer completely covers the lithium-rich manganese-based material, and the second coating layer covers a portion of the surface of the first coating layer (eg Figure 1 shown).

[0058] In one example, the first coating layer completely covers the lithium-rich manganese-based material, and the second coating layer covers the entire surface of the first coating layer (eg Figure 2 shown).

[0059] In one example, in the XRD spectrum of the positive electrode material, characteristic peaks exist at 36°-36.5° (e.g., 36°, 36.1°, 36.2°, 36.3°, 36.4°, or 36.5°) and 43.8°-44.2° (e.g., 43.8°, 43.9°, 44°, 44.1°, or 44.2°). Figure 3 and Figure 4 As shown, when characteristic peaks exist at 36°-36.5° and 43.8°-44.2°, the positive electrode material includes a spinel structure. The presence of the spinel structure can increase the ion transfer rate of the positive electrode material while inhibiting the escape of lattice oxygen in the lithium-rich manganese-based material and inhibiting irreversible phase change. Therefore, the positive electrode material has good ion conductivity, high first efficiency, good rate performance, high cycle capacity retention rate, and reduced voltage during the cycle.

[0060] The XRD analysis of the positive electrode material may be performed using the following parameters: using a Cu target, a scanning range of 15°-75°, and a scanning speed of 2° / min.

[0061] In one example, based on the total weight of the first coating layer, the weight content of the first material is 80%-100% (eg, 80%, 85%, 90%, 95% or 100%).

[0062] In one example, based on the total weight of the first coating layer, the weight content of the first material is 92%-100%.

[0063] In one example, the first coating layer further includes a lithium-rich structure and / or a rock salt phase structure.

[0064] In one example, based on the total weight of the first coating layer, the weight content of the lithium-rich structure and / or rock salt phase structure is 0%-20% (e.g., 0%, 0.1%, 0.5%, 1%, 5%, 10%, 15% or 20%).

[0065] In one example, based on the total weight of the first coating layer, the weight content of the lithium-rich structure and / or the rock salt phase structure is 0%-8%.

[0066] When the weight content of the first material in the first coating layer is 100%, the first coating layer is entirely made up of the first material, and no lithium-rich structure and / or rock salt phase structure exists.

[0067] The second coating layer may be entirely made of the second material.

[0068] The positive electrode material of the present invention can be prepared by the following method:

[0069] A precursor of a lithium-rich manganese-based material is mixed with lithium carbonate to form a mixture, the mixture is subjected to a first sintering and crushing to obtain a first crushed material, the first crushed material is mixed with an oxide material containing a fast ion conductor precursor or a carbon material containing a fast ion conductor precursor to obtain a first intermediate, and the first intermediate is subjected to a first high-temperature treatment.

[0070] The above method can be used to prepare a positive electrode material in which the second coating layer is a discontinuous coating (island coating). Figure 7 As shown, it is a SEM image of the uncoated lithium-rich manganese-based material. Figure 8 Shown is the SEM image of the island-coated cathode material.

[0071] In one example, the precursor of the lithium-rich manganese-based material includes Ni 0.40 Co 0.05 Mn 0.53 W 0.005 Nb0.015 CO3 and / or Ni 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015 (OH)2. In the present invention, the precursor of the lithium-rich manganese-based material can be obtained commercially.

[0072] In one example, the weight ratio of the precursor of the lithium-rich manganese-based material to the weight of lithium carbonate is 1:(0.42-0.52) (eg, 1:0.42, 1:0.45, 1:0.48, 1:0.5 or 1:0.52).

[0073] In one example, the first sintering conditions include: a sintering temperature of 850° C.-900° C.; a sintering time of 10 h-20 h; and a sintering atmosphere including air and / or oxygen.

[0074] In one example, the weight ratio of the first pulverized material to the oxide material containing the fast ion conductor precursor is 100:(0.4-1.2) (eg, 100:0.4, 100:0.5, 100:0.7, 100:1 or 100:1.2).

[0075] In one example, the weight ratio of the first pulverized material to the carbon material containing the fast ion conductor precursor is 100:(0.12-0.32) (for example, 100:0.12, 100:0.15, 100:0.18, 100:0.2, 100:0.22, 100:0.25, 100:0.28, 100:0.3 or 100:0.32).

[0076] In one example, the precursor of the fast ion conductor includes one or more of phosphotungstic acid, phosphoric acid, and phosphomolybdic acid.

[0077] In one example, the conditions of the first high temperature treatment include: the temperature of the high temperature treatment is 500℃-800℃ (for example, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃ or 800℃); the time of the high temperature treatment is 6h-10h (for example, 6h, 7h, 8h, 9h or 10h); the atmosphere of the high temperature treatment includes air and / or oxygen.

[0078] The positive electrode material of the present invention can also be prepared by the following method:

[0079] The precursor of the lithium-rich manganese-based material is mixed with lithium carbonate to form a mixture, the mixture is subjected to a second sintering and crushed to obtain a second crushed material, the oxide material containing the fast ion conductor precursor or the carbon material containing the fast ion conductor precursor is dispersed in a second solvent to obtain a second emulsion, the second crushed material and the second emulsion are mixed and stirred to obtain a second intermediate, and the second intermediate is subjected to a second high-temperature treatment.

[0080] The above method can be used to prepare a positive electrode material continuously coated with a second coating layer.

[0081] In one example, the precursor of the lithium-rich manganese-based material includes Ni 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015 CO3 and / or Ni 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015 (OH)2. In the present invention, the precursor of the lithium-rich manganese-based material can be obtained commercially.

[0082] In one example, the weight ratio of the precursor of the lithium-rich manganese-based material to the weight of lithium carbonate is 1:(0.42-0.52) (eg, 1:0.42, 1:0.45, 1:0.48, 1:0.5 or 1:0.52).

[0083] In one example, the second sintering conditions include: a sintering temperature of 850° C.-900° C.; a sintering time of 10 h-20 h; and a sintering atmosphere including air and / or oxygen.

[0084] In one example, the second solvent includes ethanol.

[0085] In one example, the weight ratio of the second solvent to the oxide material containing the fast ion conductor precursor is 1:(0.003-0.008) (eg, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007 or 1:0.008).

[0086] In one example, the weight ratio of the second solvent to the carbon material containing the fast ion conductor precursor is 1:(0.003-0.008) (eg, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007 or 1:0.008).

[0087] In one example, the weight ratio of the second solvent to the lithium-rich manganese-based material is (0.3-0.8):1 (eg, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1 or 0.8:1).

[0088] In one example, the stirring is continued at 60° C.-80° C. until the weight content of the second solvent is lower than 0.05% (eg, 0.045%, 0.04%, 0.03%, 0.02%, 0.01% or 0.005%).

[0089] In one example, the conditions of the second high temperature treatment include: the temperature of the high temperature treatment is 500℃-800℃ (for example, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃ or 800℃); the time of the high temperature treatment is 6h-10h (for example, 6h, 7h, 8h, 9h or 10h); the atmosphere of the high temperature treatment includes air and / or oxygen.

[0090] The positive electrode material of the present invention can be prepared by using the above two methods. In the above two methods for preparing the positive electrode material of the present invention, after the first intermediate is subjected to the first high-temperature treatment (or after the second intermediate is subjected to the high-temperature treatment), part of the lithium ions are released from the surface of the lithium-rich manganese-based material, so that the surface of the lithium-rich manganese-based material forms a lithium-deficient state, thereby transforming into a spinel structure during the high-temperature treatment process, thereby forming a first coating layer in situ on the surface of the lithium-rich manganese-based material, and the released lithium ions react with the solid acid in the oxide coating layer to form a fast ion conductor, and a second coating layer is formed on the second material outside the first coating layer to block the contact between the electrolyte and the lithium-rich manganese-based material. And before coating, the precursor of the fast ion conductor has been composited with the oxide material or the carbon material to form a whole (for example, the precursor of the fast ion conductor is embedded in the pores of the oxide material and / or the surface of the oxide material, or the precursor of the fast ion conductor is embedded in the pores of the carbon material and / or the surface of the carbon material). During the coating process, the precursor of the fast ion conductor as a whole forms a fast ion conductor in the oxide material or the carbon material and forms a second coating layer at the same time, which can reduce the interface of the solid-solid material and improve the rate performance of the positive electrode material more significantly. However, for example, the fast ion conductor is simply mixed with the oxide material. At this time, during the coating process, the fast ion conductor and the oxide material are two coated substances, and there are more solid-solid interfaces, which will affect the improvement of the rate performance of the positive electrode material.

[0091] It can be seen from the above two preparation methods that the first coating layer and the second coating layer are formed simultaneously during the preparation of the lithium-rich manganese-based material. The positive electrode material obtained in this way will form a first interface structure with no obvious boundary, in which the lithium-rich manganese-based material and the first material are intertwined and mixed, at the interface between the lithium-rich manganese-based material and the first coating layer, thereby making the lithium-rich manganese-based material and the first coating layer more tightly bonded. At the same time, a second interface structure with no obvious boundary, in which the first material and the second material are intertwined and mixed, is formed at the interface between the first coating layer and the second coating layer, thereby making the first coating layer and the second coating layer more tightly bonded, making the overall structural stability of the positive electrode material stronger, thereby improving the first efficiency and rate performance of the positive electrode material.

[0092] A second aspect of the present invention provides a positive electrode sheet, which includes the positive electrode material described in the first aspect of the present invention.

[0093] The materials of the positive electrode sheet other than the positive electrode material can be prepared in accordance with the methods in the art, and can achieve the effects of improving the battery cycle stability, rate performance and reducing the battery cycle voltage drop.

[0094] In one example, the average particle size of the positive electrode material is 6 μm-12 μm.

[0095] In the present invention, the average particle size can be obtained by laser particle size analyzer or SEM test.

[0096] In one example, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on one side or both sides of the positive electrode current collector, and the positive electrode active material layer includes the positive electrode material.

[0097] In one example, based on the total weight of the positive electrode active material layer, the weight content of the positive electrode material is 80%-96% (for example, 80%, 82%, 85%, 88%, 90%, 92%, 94%, 95% or 96%).

[0098] In one example, based on the total weight of the positive electrode active material layer, the weight content of the positive electrode material is 85%-92%.

[0099] In one example, the positive electrode active material layer further includes a positive electrode conductor and a positive electrode binder.

[0100] In one example, the positive electrode conductive agent includes at least one of acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes and metal powder.

[0101] In one example, the positive electrode binder includes at least one of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose, styrene-butadiene rubber, polytetrafluoroethylene, and polyethylene oxide.

[0102] In one example, based on the total weight of the positive electrode active material layer, the weight content of the positive electrode conductor is 2%-10% (for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%), and the weight content of the positive electrode binder is 2%-10% (for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%).

[0103] In one example, based on the total weight of the positive electrode active material layer, the weight content of the positive electrode conductor is 4%-7.5%, and the weight content of the positive electrode binder is 4%-7.5%.

[0104] In one example, the compaction density of the positive electrode sheet is 2.8 g / cm 3 -3g / cm 3 (For example, 2.8 g / cm 3 , 2.82g / cm 3 , 2.85g / cm 3 , 2.88g / cm 3 , 2.9g / cm 3 , 2.92g / cm 3 , 2.95g / cm 3 , 2.98g / cm 3 or 3g / cm 3 ).

[0105] The positive electrode sheet of the present invention includes the positive electrode material of the present invention, thereby improving the cycle stability and rate performance of the battery and reducing the voltage drop of the battery.

[0106] A third aspect of the present invention provides a battery, comprising the positive electrode sheet described in the second aspect of the present invention.

[0107] The materials of the battery except the negative electrode sheet can be made according to the methods in the art, and can achieve the effects of improving cycle stability, rate performance and reducing cycle voltage drop.

[0108] In one example, the battery is a lithium-ion battery.

[0109] In one example, the battery is a lithium-ion secondary battery.

[0110] In one example, the battery further includes a negative electrode sheet, an electrolyte, and a separator.

[0111] The negative electrode sheet may be a conventional negative electrode sheet in the art, for example, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on one side or both sides of the negative electrode current collector, and the negative electrode active material layer includes a negative electrode material, a negative electrode conductor and a negative electrode binder.

[0112] In one example, the negative electrode material includes one or more of graphite, silicon carbon, and silicon oxygen.

[0113] In one example, the negative electrode conductive agent includes at least one of acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes and metal powder.

[0114] In one example, the negative electrode binder includes at least one of styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid, polyvinyl alcohol, and polyvinylidene fluoride.

[0115] In one example, based on the total weight of the negative electrode active material layer, the weight content of the negative electrode material is 80%-96% (for example, 80%, 82%, 85%, 88%, 90%, 92%, 95% or 96%), the weight content of the negative electrode conductor is 2%-10% (for example, 2%, 5%, 8% or 10%), and the weight content of the negative electrode binder is 2%-10% (for example, 2%, 5%, 8% or 10%).

[0116] In one example, based on the total weight of the negative electrode active material layer, the weight content of the negative electrode material is 85%-92%, the weight content of the negative electrode conductor is 4%-7.5%, and the weight content of the negative electrode binder is 4%-7.5%.

[0117] The electrolyte may be a conventional electrolyte in the art, for example, the electrolyte includes a lithium salt, an organic solvent and an additive.

[0118] In one example, the lithium salt includes one or more of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium bisfluorosulfonyl imide (LiTFSI), lithium bistrifluoromethylsulfonyl imide, lithium difluorobisoxalatophosphate, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium and lithium bis(trifluoromethylsulfonyl)imide.

[0119] In one example, the organic solvent includes one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC).

[0120] In one example, the additive includes one or more of vinylene carbonate (VC), 1,3-propane sultone (PS), 1,3-acrylonitrile lactone (PST), vinyl ethylene carbonate (VEC), succinonitrile (SN) and 1,3,6-hexanetrinitrile (HTCN).

[0121] In one example, based on the total weight of the electrolyte, the weight content of the lithium salt is 8%-15% (for example, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%), the weight content of the organic solvent is 78%-88% (for example, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87% or 88%), and the weight content of the additive is 3%-10% (for example, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%).

[0122] In one example, based on the total weight of the electrolyte, the weight content of the lithium salt is 10%-12%, the weight content of the organic solvent is 80%-85%, and the weight content of the additive is 5%-8%.

[0123] The diaphragm may be a conventional diaphragm in the art, for example, the diaphragm comprises a substrate layer and a coating located on at least one surface of the substrate layer, wherein the coating comprises a ceramic layer and / or a rubber coating layer.

[0124] In one example, the substrate layer is made of at least one of polyethylene, polypropylene, a composite material of polyethylene and polypropylene, polyamide, polyimide, and aramid.

[0125] In one example, the ceramic layer includes inorganic particles and a separator binder.

[0126] In one example, based on the total weight of the ceramic layer, the weight content of the inorganic particles is 80%-99% (e.g., 80%, 85%, 90%, 95% or 99%), and the weight content of the diaphragm adhesive is 1%-20% (e.g., 1%, 5%, 10%, 15% or 20%).

[0127] In one example, the inorganic particles include at least one of aluminum oxide, magnesium oxide, boehmite, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide, and nickel oxide.

[0128] In one example, the membrane adhesive includes at least one of polyacrylate, polytetrafluoroethylene, polyvinylidene fluoride, hexafluoropropylene-vinylidene fluoride copolymer (eg, polyvinylidene fluoride-hexafluoropropylene copolymer), polyimide, polyacrylonitrile, and polymethyl methacrylate.

[0129] In one example, the coating layer includes a polymer, and the monomer of the polymer includes at least one of styrene, vinyl chloride, perfluoropropylene, chlorotrifluoroethylene, tetrafluoroethylene, vinylidene chloride, tetrachloroethylene, acrylate (for example, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate), methacrylic acid, methacrylate (for example, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate), and acrylonitrile.

[0130] The battery of the present invention comprises the positive electrode material and the positive electrode sheet of the present invention, thereby improving the initial efficiency, the cycle stability and the rate performance, and reducing the voltage drop of the cycle voltage.

[0131] The present invention will be described in detail below by way of examples. The examples described in the present invention are only a part of the examples of the present invention, rather than all of the examples. Based on the examples in the present invention, all other examples obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0132] The following examples are used to illustrate the positive electrode material and positive electrode sheet of the present invention.

[0133] Example 1

[0134] (1) Preparation of positive electrode materials

[0135] The precursor of the lithium-rich manganese-based material is mixed with lithium carbonate to form a mixture, the mixture is subjected to a second sintering and crushed to obtain a second crushed material, the oxide material containing the fast ion conductor precursor is dispersed in a second solvent to obtain a second emulsion, the second crushed material and the second emulsion are mixed and heated and stirred to evaporate the solvent to obtain a second intermediate, and the second intermediate is subjected to a second high-temperature treatment.

[0136] Wherein, the precursor of the lithium-rich manganese-based material is Ni 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015 CO3; the precursor of the fast ion conductor is phosphotungstic acid; the second solvent is ethanol; the weight ratio of the precursor of the lithium-rich manganese-based material to the weight of lithium carbonate is 1:0.47; the weight ratio of the second solvent to the oxide material containing the fast ion conductor precursor is 1:0.005, and the weight ratio of the second solvent to the lithium-rich manganese-based material is 0.5:1;

[0137] The conditions for the second sintering include: a sintering temperature of 880°C; a sintering time of 12 hours; a sintering atmosphere of air; stirring is continuous stirring at 80°C until the weight content of the second solvent is 0.003%; the conditions for the second high-temperature treatment include: a high-temperature treatment temperature of 700°C, a high-temperature treatment time of 8 hours; and a high-temperature treatment atmosphere of air.

[0138] (2) Preparation of positive electrode

[0139] Positive electrode material: 80 parts by weight;

[0140] Positive electrode conductive agent: acetylene black, 10 parts by weight;

[0141] Positive electrode binder: PVDF, 10 parts by weight.

[0142] The positive electrode material, positive electrode conductor and positive electrode binder were mixed in 10 ml of N-methylpyrrolidone and stirred thoroughly to form positive electrode slurry. The positive electrode slurry was then coated on one surface of the aluminum foil by a coating machine and dried to obtain a positive electrode sheet.

[0143] Example 2

[0144] (1) Preparation of positive electrode materials

[0145] The precursor of the lithium-rich manganese-based material is mixed with lithium carbonate to form a mixture, the mixture is first sintered and crushed to obtain a first crushed material, the first crushed material is mixed with an oxide material containing a fast ion conductor precursor to obtain a first intermediate, and the first intermediate is subjected to a first high-temperature treatment.

[0146] Wherein, the precursor Ni of the lithium-rich manganese-based material 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015 CO3; the precursor of the fast ion conductor is phosphotungstic acid; the weight ratio of the precursor of the lithium-rich manganese-based material to the weight ratio of lithium carbonate is 1:0.47; the weight ratio of the first crushed material to the oxide material containing the fast ion conductor precursor is 100:0.25;

[0147] The conditions for the first sintering include: a sintering temperature of 880° C.; a sintering time of 12 hours; and an air sintering atmosphere; the conditions for the first high-temperature treatment include: a high-temperature treatment temperature of 700° C.; a high-temperature treatment time of 8 hours; and an air atmosphere for the high-temperature treatment.

[0148] (2) Preparation of positive electrode

[0149] The preparation of the positive electrode sheet is carried out with reference to Example 1.

[0150] Example 3 Group

[0151] This group of examples is used to illustrate the effects produced when the fast ion conductor is changed.

[0152] This group of examples is carried out with reference to Example 1, except that the specific selection of the fast ion conductor is changed, as shown in Table 1.

[0153] Example 4 Group

[0154] This group of examples is used to illustrate the effects produced when the oxide material is changed.

[0155] This group of examples is carried out with reference to Example 1, except that the specific selection of oxide materials is changed, see Table 1 for details.

[0156] Example 5 Group

[0157] This group of examples is used to illustrate the influence produced when the oxide material is changed to a carbon material.

[0158] This group of examples is carried out with reference to Example 2, except that the oxide material is adjusted to a carbon material, see Table 1 for details.

[0159] Example 6

[0160] The process is carried out in accordance with Example 1, except that the weight content of the first material in the first coating layer and the weight content of the fast ion conductor in the oxide material containing the fast ion conductor are changed. For details, see Table 1.

[0161] Example 7 Group

[0162] This group of examples is used to illustrate the effects produced when the weight content of the fast ion conductor in the fast ion conductor-containing oxide material is changed.

[0163] This group of examples is carried out with reference to Example 1, except that the weight content of the fast ion conductor in the oxide material containing the fast ion conductor is changed, as shown in Table 1. It can be understood that changing the weight content of the fast ion conductor in the oxide material containing the fast ion conductor will correspondingly change the thickness of the first coating layer.

[0164] Example 8 Group

[0165] This group of examples is used to illustrate the effects produced when the weight content of the fast ion conductor in the fast ion conductor-containing carbon material is changed.

[0166] This group of examples is carried out with reference to Example 5a, except that the weight content of the fast ion conductor in the carbon material containing the fast ion conductor is changed, as specifically shown in Table 1. It can be understood that changing the weight content of the fast ion conductor in the carbon material containing the fast ion conductor will correspondingly change the thickness of the first coating layer.

[0167] Comparative Example 1

[0168] The process is carried out in accordance with Example 1, except that the oxide material containing the fast ion conductor is adjusted so that the oxide material and the fast ion conductor are directly mixed. For details, see Table 1.

[0169] Comparative Example 2

[0170] Refer to Example 1, except that the oxide material containing the fast ion conductor precursor is replaced by an oxide material containing a fast ion conductor, that is, the alumina material embedded with phosphotungstic acid is directly replaced with an alumina material embedded with lithium phosphotungstate. At this time, the positive electrode material obtained does not have the first coating layer, but only the second coating layer exists.

[0171] Comparative Example 3

[0172] The precursor Ni of lithium-rich manganese-based materials 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015 CO3 and lithium carbonate are uniformly mixed in a weight ratio of 1:0.40, and then sintered at 880°C in an air atmosphere for 12 hours and then sieved to obtain an embedded spinel structure lithium-rich manganese-based positive electrode material.

[0173] 0.1 g CF y Dispersed in 50 mL NMP, ball milled at 400 r / min for 6 h, then added 9.9 g of the above-mentioned embedded spinel structure lithium-rich manganese-based positive electrode material, ball milled at 100 r / min for 2 h to mix evenly, evaporated the solvent, and then heat treated at 250 ° C for 2 h to obtain CF y Coated lithium-rich manganese-based positive electrode material with embedded spinel structure.

[0174] A positive electrode sheet was prepared according to Example 1. A button cell was assembled according to the subsequent button cell manufacturing method, and the positive electrode material was activated by charging and discharging once at 2.0-4.8V using a current of 15 mA / g. After activation, a lithium-rich manganese-based positive electrode material with an embedded spinel structure coated with a double conductive layer was obtained (the thickness of the double conductive coating layer was 7.8 nm, and the characteristic peaks of the spinel structure in the XRD spectrum of the lithium-rich manganese-based positive electrode material with an embedded spinel structure coated with a double conductive layer were located at 36.2 and 44.03).

[0175] Comparative Example 4

[0176] The precursor Ni of lithium-rich manganese-based materials 0.40 Co 0.05 Mn 0.53 W 0.005 Nb 0.015CO3 was dispersed in water at a solid-liquid mass ratio of 1:1.2, and nickel sulfate was added. After mixing and stirring, ammonia water was added dropwise until the pH value was 11. After reacting for 30 minutes, the reaction liquid was filtered and the obtained solid was dried at 80°C for 12 hours. The amount of nickel sulfate added was 1% of the mass of the precursor.

[0177] The precursor obtained above was evenly mixed with lithium carbonate in a weight ratio of 1:0.47, and then sintered at 880° C. in an air atmosphere for 12 hours and then sieved to obtain a surface nickel-rich, lithium-rich, manganese-based positive electrode material.

[0178] After ammonium molybdate and the surface nickel-rich and lithium-rich manganese-based positive electrode material are uniformly mixed, they are sintered at 800°C for 6 hours in an air atmosphere to obtain a secondary sintered material, wherein the amount of ammonium molybdate used is 1wt% of the surface nickel-rich and lithium-rich manganese-based positive electrode material.

[0179] The secondary sintered material was added to ethanol at a mass ratio of 2:1, and perfluorooctyl triethoxysiloxane was added at the same time, and stirred at 80°C until the solution evaporated, and dried in an oven to obtain an intermediate 1, wherein the amount of perfluorooctyl triethoxysiloxane was 1wt% of the secondary sintered material. The intermediate 1 was then mixed evenly with methyl pyridinium phosphate at a mixing rate of 1800rpm, wherein the amount of methyl pyridinium phosphate was 1wt% of the intermediate 1; the mixing time was 15min, and the mixture was sintered at 350°C for 4 hours in an air atmosphere to obtain a lithium-rich manganese-based positive electrode material with a continuous coating double coating layer (wherein the first coating layer was a fast ion conductor lithium molybdate with a thickness of 12.2nm and the second coating layer was a carbon layer containing fluorine and phosphorus with a thickness of 9.8nm).

[0180] Table 1

[0181]

[0182]

[0183] *Same as Example 1;

[0184] - means it does not exist.

[0185] Preparation Example

[0186] The positive electrode sheets obtained in the embodiment and the comparative example were used to prepare button-type batteries according to the following methods.

[0187] (1) Positive electrode

[0188] The positive electrode sheets obtained in the above-mentioned embodiments and comparative examples were used respectively.

[0189] (2) Negative electrode

[0190] Lithium tablets

[0191] (3) Electrolyte

[0192] Lithium salt: 12 parts by weight of lithium hexafluorophosphate, organic solvent: 83 parts by weight of ethylene carbonate (EC), additive: 5 parts by weight of vinylene carbonate (VC);

[0193] In a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm), the organic solvent and the additive are mixed evenly, and then fully dried lithium salt is quickly added thereto and stirred for 10 hours to fully dissolve it, thereby obtaining the desired electrolyte.

[0194] (4) Diaphragm

[0195] The diaphragm is based on polyethylene, with one side coated with polytetrafluoroethylene and the other side coated with alumina ceramic.

[0196] (5) Preparation of button cells

[0197] The positive electrode sheet of step (1), the negative electrode sheet of step (2), the electrolyte of step (3) and the diaphragm of step (4) are assembled into a button battery using a 2032 button battery shell in an argon-protected glove box.

[0198] Test Case

[0199] The button cells prepared in the examples and comparative examples were tested as follows:

[0200] At room temperature (25°C), charge the battery to 4.6V at 0.1C, record the charging capacity at this time as the first charging capacity, and then discharge it to 2V at 0.1C, record the released capacity as the first discharge capacity, first discharge efficiency = first discharge capacity / first charging capacity;

[0201] Then charge to 4.7V at 0.1C, and then discharge to 2V at 0.1C. The discharged capacity is recorded as the secondary discharge capacity.

[0202] Then charge to 4.8V at 0.1C, and discharge to 2V at 0.1C. The discharged capacity is recorded as the three-discharge capacity.

[0203] Then charge to 4.6V at 0.2C, and then discharge to 2V at 0.2C. The discharged capacity is recorded as 0.2C discharge capacity.

[0204] Then charge to 4.6V at 0.5C, and then discharge to 2V at 0.5C. The discharged capacity is recorded as 0.5C discharge capacity. This cycle is repeated 100 times. The discharge capacity of the 100th cycle is recorded as Q100. The capacity retention rate after 100 cycles = Q100 / 0.5C discharge capacity × 100%.

[0205] The discharge voltage drop after 100 cycles = (discharge median voltage at the first cycle - discharge median voltage at the 100th cycle) / 100.

[0206] Table 2

[0207]

[0208]

[0209] It can be seen from Table 2 that the comparative examples and embodiments show that the first discharge efficiency of the battery made of the positive electrode material of the embodiment is improved, the 0.2C / 0.1C discharge capacity is improved, the 0.5C / 0.1C discharge capacity is improved, the capacity retention rate after 100 cycles is significantly improved, and the discharge voltage drop after 100 cycles is significantly reduced, indicating that the lithium-rich manganese-based material is coated with spinel and oxide materials and carbon materials containing fast ion conductors to form a tightly bonded coating layer, which improves the stability of the positive electrode sheet, improves the first efficiency and rate performance of the battery, improves the cycle stability of the battery, and reduces the cycle voltage drop of the battery.

[0210] The battery prepared with the positive electrode material of Comparative Example 3 has poor cycle stability and a large cycle voltage drop. The reason is that the spinel structure of the positive electrode material prepared in Comparative Example 3 is embedded in the structure of the lithium-rich manganese-based material, which is not conducive to inhibiting the escape of lattice oxygen in the lithium-rich manganese-based material. Therefore, the battery prepared with it has poor cycle stability and a large cycle voltage drop.

[0211] The battery prepared with the positive electrode material of Comparative Example 4 has low 0.2C / 0.1C discharge capacity and 0.5C / 0.1C discharge capacity, and poor rate performance. The reason is that the first coating layer containing the fast ion conductor of the positive electrode material prepared in Comparative Example 4 is coated with a layer of carbon material on the outside. Lithium ions need to pass through two solid-solid interface layers to escape from the surface of the lithium-rich manganese-based material, which will greatly increase the transmission resistance of lithium ions, resulting in limited improvement in the transmission rate of lithium ions, thereby limiting the improvement in rate performance.

[0212] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A positive electrode material, It is characterized in that The positive electrode material comprises a lithium-rich manganese-based material, a first material and a second material, wherein the first material comprises a spinel structure, and the second material comprises an oxide material containing a fast ion conductor and / or a carbon material containing a fast ion conductor; The first material forms a first coating layer on the surface of the lithium-rich manganese-based material, and the second material is coated on the surface of the first coating layer to form a second coating layer. In the second coating layer, the fast ion conductor is located inside and / or on the surface of the oxide material and / or the carbon material.

2. The positive electrode material according to claim 1, in, The thickness of the second coating layer is greater than or equal to the thickness of the first coating layer; And / or, the first interface between the first coating layer and the lithium-rich manganese-based material is an interface structure in which the first material and the lithium-rich manganese-based material are interwoven and mixed; And / or, the second interface between the second coating layer and the first coating layer is an interface structure in which the second material and the first material are interwoven and mixed; And / or, the first coating layer is a coating layer formed in situ on the surface of the lithium-rich manganese-based material.

3. The positive electrode material according to claim 1, in, The ratio of the thickness of the first coating layer to the thickness of the second coating layer is 1:(1-5); And / or, based on the total weight of the oxide material containing the fast ion conductor, the weight content of the fast ion conductor is 10%-20%, preferably 13%-17%; And / or, based on the total weight of the carbon material containing the fast ion conductor, the weight content of the fast ion conductor is 10%-20%, preferably 13%-17%; And / or, the thickness of the first coating layer is 2nm-8nm; And / or, the thickness of the second coating layer is 2nm-10nm.

4. The positive electrode material according to claim 1, in, The first coating layer completely covers the lithium-rich manganese-based material; And / or, the second coating layer covers part or all of the surface of the first coating layer.

5. The positive electrode material according to claim 1, in, Based on the total weight of the first coating layer, the weight content of the first material is 80%-100%; And / or, the second coating layer is entirely made of the second material.

6. The positive electrode material according to claim 1, in, The fast ion conductor includes one or more of lithium phosphotungstate, lithium phosphate and lithium phosphomolybdate; and / or, the oxide material comprises one or more of zirconium dioxide, titanium dioxide, aluminum oxide and silicon dioxide; and / or, the carbon material comprises one or more of activated carbon, graphite and carbon nanotubes; And / or, the lithium-rich manganese-based material comprises a chemical formula of xLi 2 MnO 3 ·(1-x)LiNi a Co b Mn c O 2 Particles, where 0<x<1, 0≤a≤1, 0≤b≤1, 0≤c≤1, a+b+c=1.

7. The positive electrode material according to any one of claims 1 to 6, in, The oxide material has a porous structure, and the fast ion conductor is embedded in the pores of the oxide material; And / or, the carbon material has a porous structure, and the fast ion conductor is embedded in the pores of the carbon material; And / or, in the XRD spectrum of the positive electrode material, characteristic peaks exist at 36°-36.5° and 43.8°-44.2°.

8. A positive electrode sheet, It is characterized in that The positive electrode sheet comprises the positive electrode material according to any one of claims 1 to 7.

9. The positive electrode sheet according to claim 8, in, The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on one side or both sides of the positive electrode current collector, wherein the positive electrode active material layer comprises the positive electrode material, and the weight content of the positive electrode material is 80%-96% based on the total weight of the positive electrode active material layer; And / or, the average particle size of the positive electrode material is 6 μm-12 μm; And / or, the compaction density of the positive electrode sheet is 2.8 g / cm 3 -3g / cm 3 .

10. A battery, It is characterized in that The battery comprises the positive electrode sheet according to claim 8 or 9.

Citation Information

Cited By

  • Lithium-rich manganese-based positive electrode material with core-shell structure and preparation method of lithium-rich manganese-based positive electrode material

    CN121726383A

  • A core-shell structure lithium-rich manganese-based positive electrode material and a preparation method thereof

    CN121726383B

  • Lithium-ion secondary battery, positive electrode sheet, positive electrode active material, method for preparing positive electrode active material, and electrical apparatus

    WO2026144268A1