Lithium-sulfur battery composite modified diaphragm, preparation method and battery comprising lithium-sulfur battery composite modified diaphragm
By coating Cu-Ni/MOF nanoparticles on the surface of the polyacrylonitrile nanofiber matrix of lithium sulfur batteries, a composite modified separator was prepared, which solved the problems of polysulfide shuttle effect and lithium dendrites in lithium sulfur batteries, and improved the Coulombic efficiency, cycle stability and safety of the battery.
Patent Information
- Application Number
- CN202411228487.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
AI Technical Summary
In practical applications, lithium sulfur batteries face the "shuttle effect" of polysulfide and the growth of lithium dendrites, resulting in insufficient electrochemical performance and safety. The existing diaphragm modification methods are not effective and cannot effectively inhibit the shuttle of polysulfides. Effects and enhance safety.
Using polyacrylonitrile nanofiber matrix as the basis, diatom Cu-Ni/MOF nanoparticles are coated, and composite modified separators are prepared through electrospinning technology to improve the capture and conversion efficiency of polysulfides, and enhance the Coulomb efficiency and circulation of the battery. Stability and safety.
Through the synergistic catalysis of Cu-Ni/MOF nanoparticles, polysulfides can be effectively captured and converted, shuttle effect can be reduced, cycle stability and safety of the battery, and the Coulomb efficiency and high rate performance of the battery can be improved.
Smart Images

Figure CN119050600A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-sulfur batteries, and in particular to a lithium-sulfur battery composite modified diaphragm and a preparation method thereof, and a battery comprising the same. Background Art
[0002] Lithium-sulfur battery (LSB) is a popular battery due to its high energy density (theoretical specific capacity is 1675mAh g ^-1 ), low cost and environmental friendliness, etc., and has attracted widespread attention in recent years. However, LSB still faces many challenges in practical applications, mainly including the "shuttle effect" of polysulfide and the growth of lithium dendrites. Therefore, the electrochemical performance and safety of LSB need to be improved.
[0003] The "shuttle effect" of polysulfides refers to the process in which polysulfides (Li2S n, 2 ≤n ≤ 8) dissolves in the electrolyte and diffuses to the lithium negative electrode, reacting with lithium to form precipitated Li2S or Li2S2, which not only leads to the loss of active materials, but also causes serious self-discharge inside the battery, reducing the coulombic efficiency and cycle life of the battery. In related technologies, there are methods such as electrolyte modification, cathode material modification, diaphragm modification, and interface engineering to inhibit the "shuttle effect" of polysulfide compounds. Due to the limitations of the diaphragm in electrolyte absorption and polysulfide capture space, the effect of inhibiting the "shuttle effect" of polysulfide compounds is not good, and it also cannot solve the safety problems of lithium-sulfur batteries.
[0004] Therefore, it is necessary to provide a solution for a lithium-sulfur battery composite modified diaphragm to improve the comprehensive performance of lithium-sulfur batteries. Summary of the invention
[0005] In view of this, the present application provides a lithium-sulfur battery composite modified diaphragm and a preparation method, and a battery containing the same, which are used to solve the problem of poor overall performance of lithium-sulfur batteries.
[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a lithium-sulfur battery composite modified diaphragm, which includes a polyacrylonitrile nanofiber matrix and Cu-Ni / MOF nanoparticles coated on the surface of the polyacrylonitrile nanofiber matrix.
[0007] Preferably, the porosity of the polyacrylonitrile nanofiber matrix is 60-65%, and the average pore diameter of the polyacrylonitrile nanofiber matrix is 20-25 nm.
[0008] In a second aspect, the present application provides a method for preparing a composite modified diaphragm for a lithium-sulfur battery, comprising the following steps: S1. Obtaining Cu-Ni / MOF nanoparticles; S2. Using polyacrylonitrile solution as raw material, preparing polyacrylonitrile nanofiber matrix by electrospinning process; S3. dispersing the Cu-Ni / MOF nanoparticles in a solvent, and then coating the Cu-Ni / MOF nanoparticles on the surface of the polyacrylonitrile nanofiber substrate to obtain a nanofiber membrane; S4. Drying the nanofiber membrane to obtain the lithium-sulfur battery composite modified membrane.
[0009] Preferably, in step S1, the preparation method of Cu-Ni / MOF nanoparticles is: adding Ni(NO3)2·6H2O and Cu(NO3)2·3H2O to a mixture of anhydrous ethanol, pure water and DMF to obtain an intermediate product, then adding BTC to the intermediate product, heating to react, filtering, washing and drying the precipitate to obtain Cu-Ni / MOF nanoparticles.
[0010] Preferably, the volume ratio of anhydrous ethanol, pure water and DMF is 1:1:1-2.
[0011] Preferably, the mass ratio of Ni(NO3)2·6H2O to Cu(NO3)2·3H2O is 1:1-2.
[0012] Preferably, the heating reaction temperature is 160-170° C., and the heating reaction time is 4-8 h.
[0013] Preferably, in step S3, the thickness ratio of the Cu-Ni / MOF nanoparticles to the polyacrylonitrile nanofiber matrix is 0.1-1:2.
[0014] Preferably, the process conditions of the electrospinning are: solution concentration 10-15%, spray voltage 18-20KV, receiving distance 120-140mm, solution propulsion speed 0.025-0.03ml / min, and needle diameter 0.8-0.9mm.
[0015] In a third aspect, the present application provides a lithium-sulfur battery, which includes a lithium-sulfur battery composite modified diaphragm.
[0016] The beneficial effects of the present application are as follows: the present application coats diatomic Cu-Ni / MOF nanoparticles on the surface of the polyacrylonitrile nanofiber substrate so that the diatomic Cu-Ni / MOF nanoparticles are evenly distributed on the surface of the polyacrylonitrile nanofiber substrate, which is beneficial to the improvement of the sites and spaces for capturing and converting polysulfides by the composite modified diaphragm of the lithium-sulfur battery, and the efficiency of capturing and converting polysulfides is enhanced to reduce the shuttling effect of polysulfides, and ultimately improve the coulombic efficiency, capacity retention rate and cycle stability of the lithium-sulfur battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is an identification diagram of each material obtained in Example 1. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0019] The present application provides a lithium-sulfur battery composite modified diaphragm, which includes a polyacrylonitrile nanofiber matrix and Cu-Ni / MOF nanoparticles coated on the surface of the polyacrylonitrile nanofiber matrix.
[0020] In the present application, diatomic Cu-Ni / MOF nanoparticles are coated on the surface of the polyacrylonitrile nanofiber matrix so that the diatomic Cu-Ni / MOF nanoparticles are evenly distributed on the surface of the polyacrylonitrile nanofiber matrix, which is beneficial for the lithium-sulfur battery composite modified diaphragm to capture and convert polysulfides, and the efficiency of capturing and converting polysulfides is enhanced to reduce the shuttling effect of polysulfides, and ultimately improve the coulombic efficiency, capacity retention rate and cycle stability of the lithium-sulfur battery.
[0021] Among them, the diatomic Cu-Ni / MOF nanoparticles have the function of synergistically catalyzing the adsorption of polysulfides, realizing the physical capture and chemical adsorption of polysulfides, and improving the adsorption and catalytic conversion efficiency of polysulfides, and reducing the shuttling effect of polysulfides. At the same time, the diatomic Cu-Ni / MOF nanoparticles of the present application have strong chemical adsorption and catalytic conversion of polysulfide compounds, which can improve the discharge capacity and cycle life of the battery at high rate, taking into account the high rate performance and cycle life of the battery; the porosity and pore size of the polyacrylonitrile nanofiber matrix are adjustable, which is conducive to the absorption of electrolytes and ion conduction; the diatomic Cu-Ni / MOF nanoparticles coated on the polyacrylonitrile nanofiber matrix can make each pore of the polyacrylonitrile nanofiber have sufficient active sites to capture and convert polysulfides to reduce the shuttling effect of polysulfides; therefore, the coulombic efficiency and cycle stability of the lithium battery are improved by reducing the shuttling effect of polysulfides.
[0022] Furthermore, by coating the surface of the polyacrylonitrile nanofiber substrate with diatomic Cu-Ni / MOF nanoparticles having high ionic conductivity and electrolyte absorption, it helps to evenly distribute the current density and inhibit the growth of lithium dendrites; at the same time, coating the surface of the polyacrylonitrile nanofiber substrate with diatomic Cu-Ni / MOF nanoparticles improves the mechanical strength of the polyacrylonitrile nanofiber substrate to inhibit the growth of lithium dendrites in the battery; therefore, the lithium-sulfur battery composite modified diaphragm of the present application improves the safety of the battery through the growth of lithium dendrites.
[0023] In some embodiments, the porosity of the polyacrylonitrile nanofiber matrix is 60-65%, and the average pore diameter of the polyacrylonitrile nanofiber matrix is 20-25 nm.
[0024] In this embodiment, the polyacrylonitrile nanofiber matrix is within this porosity range, and the lithium-sulfur battery composite modified diaphragm has strong mechanical strength, good ion conductivity and electrolyte absorption, and provides sufficient sites for capturing polysulfides.
[0025] The present application provides a method for preparing a composite modified diaphragm for a lithium-sulfur battery, comprising the following steps: S1. Obtaining Cu-Ni / MOF nanoparticles; S2. Using polyacrylonitrile solution as raw material, preparing polyacrylonitrile nanofiber matrix by electrospinning process; S3. dispersing the Cu-Ni / MOF nanoparticles in a solvent, and then coating the Cu-Ni / MOF nanoparticles on the surface of the polyacrylonitrile nanofiber substrate to obtain a nanofiber membrane; S4. Drying the nanofiber membrane to obtain the lithium-sulfur battery composite modified membrane.
[0026] In the present application, the polyacrylonitrile nanofiber matrix prepared by electrospinning technology has the advantages of high porosity and adjustable pore size, which not only improves the electrolyte absorption capacity and ion conduction efficiency, but also provides sufficient loading space for MOF nanoparticles, which is beneficial to the effective capture and conversion of polysulfides.
[0027] In some embodiments, in step S1, the preparation method of Cu-Ni / MOF nanoparticles is: adding Ni(NO3)2·6H2O and Cu(NO3)2·3H2O to a mixture of anhydrous ethanol, pure water and DMF to obtain an intermediate product, then adding BTC to the intermediate product, heating to react, filtering, washing and drying the precipitate to obtain Cu-Ni / MOF nanoparticles.
[0028] In this embodiment, the above method is used to form a MOFS material centered on diatomic Cu-Ni, which is beneficial to the synergistic catalytic adsorption of Cu and Ni.
[0029] In some embodiments, the volume ratio of anhydrous ethanol, pure water and DMF is 1:1:1-2.
[0030] In some embodiments, the mass ratio of Ni(NO3)2·6H2O to Cu(NO3)2·3H2O is 1:1-2.
[0031] In some embodiments, the heating reaction temperature is 160-170° C., and the heating reaction time is 4-8 hours.
[0032] In this embodiment, by controlling the above process conditions, the uniformity and stability of Cu-Ni / MOF nanoparticles can be improved, so that the Cu-Ni / MOF nanoparticles can play a role in the diaphragm with lasting stability. Specifically, controlling the ratio of metal precursors, ligand concentration, reaction temperature, reaction time, solvent selection and stirring rate is crucial to improving the uniformity and stability of particles. Accurately controlling the concentration of metal precursors and ligands can ensure uniform distribution of metal ions, optimizing reaction temperature and time helps to form a stable framework structure, and selecting suitable solvents and stirring rates can effectively prevent particle aggregation, ensuring that the final product has good uniformity and stability.
[0033] In some embodiments, in step S2, in the electrospinning process, the solution concentration is 10-15%, the injection voltage is 18-20KV, the receiving distance is 120-140mm, the solution propulsion speed is 0.025-0.03ml / min, and the needle diameter is 0.8-0.9mm.
[0034] In some embodiments, in step S3, the thickness ratio of the Cu-Ni / MOF nanoparticles to the polyacrylonitrile nanofiber matrix is 0.1-1:2.
[0035] In this embodiment, by controlling the above conditions, it is ensured that there are sufficient Cu-Ni / MOF nanoparticles on the polyacrylonitrile nanofiber matrix.
[0036] In this embodiment, by controlling the above process conditions, the overall strength and stability of the composite modified separator of the lithium-sulfur battery can be improved, and the safety of the lithium-sulfur battery can be correspondingly improved.
[0037] In a third aspect, the present application provides a lithium-sulfur battery, which includes a lithium-sulfur battery composite modified diaphragm.
[0038] In the present application, the lithium-sulfur battery includes a lithium-sulfur battery composite modified diaphragm, which improves the discharge capacity, capacity retention rate at high rate, cycle stability, coulombic efficiency and safety of the lithium-sulfur battery.
[0039] The present solution is further described below through specific embodiments.
[0040] Example 1 A method for preparing a composite modified diaphragm for a lithium-sulfur battery comprises the following steps: S1. Add Ni(NO3)2·6H2O and Cu(NO3)2·3H2O to a mixture of anhydrous ethanol, pure water and DMF to obtain an intermediate product, then add BTC to the intermediate product, heat at 170°C for 6 hours, filter, wash and dry the precipitate to obtain Cu-Ni / MOF nanoparticles; wherein the volume ratio of anhydrous ethanol, pure water and DMF is 1:1:1; the mass ratio of Ni(NO3)2·6H2O to Cu(NO3)2·3H2O is 1:1; S2. Using polyacrylonitrile solution as raw material, polyacrylonitrile nanofiber matrix was prepared by electrospinning process; the process conditions of electrospinning were: solution concentration 12%, spray voltage 18KV, receiving distance 120-140mm, solution propulsion speed 0.027ml / min, needle diameter 0.86mm; S3. Dispersing the Cu-Ni / MOF nanoparticles in a solvent, and then coating the Cu-Ni / MOF nanoparticles on the surface of the polyacrylonitrile nanofiber substrate to obtain a nanofiber membrane; wherein the thickness ratio of the Cu-Ni / MOF nanoparticles to the polyacrylonitrile nanofiber substrate is 1:2; S4. Dry the nanofiber membrane to obtain the lithium-sulfur battery composite modified membrane.
[0041] The lithium-sulfur battery composite modified diaphragm obtained according to the above preparation method includes a polyacrylonitrile nanofiber matrix and Cu-Ni / MOF nanoparticles coated on the surface of the polyacrylonitrile nanofiber matrix; the porosity of the polyacrylonitrile nanofiber matrix is 62%, and the average pore diameter of the polyacrylonitrile nanofiber matrix is 22nm.
[0042] Example 2 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, the other contents of which are the same as those of Example 1, except that the mass ratio of Ni(NO3)2·6H2O to Cu(NO3)2·3H2O is 1:2.
[0043] Example 3 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, wherein other contents are the same as those of Example 1, except that the thickness ratio of the Cu-Ni / MOF nanoparticles to the polyacrylonitrile nanofiber matrix is 0.1:2.
[0044] Example 4 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, the other contents of which are the same as those of Example 1, except that the heating temperature in step S1 is 180°C.
[0045] Comparative Example 1 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, the other contents are the same as those in Example 1, except that the Cu-Ni / MOF nanoparticles are replaced by Cu / MOF nanoparticles.
[0046] Comparative Example 2 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, the other contents of which are the same as those of Example 1, except that the Cu-Ni / MOF nanoparticles are replaced by Ni / MOF nanoparticles.
[0047] Comparative Example 3 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, the other contents of which are the same as those of Example 1, except that the Cu-Ni / MOF nanoparticles are replaced by MOF nanoparticles.
[0048] Comparative Example 4 A method for preparing a composite modified diaphragm for a lithium-sulfur battery, the other contents are the same as those in Example 1, except that the Cu-Ni / MOF nanoparticles are replaced by Co-Ni / MOF.
[0049] Test and Evaluation The lithium-sulfur battery composite modified diaphragms obtained in the embodiments and comparative examples were prepared into lithium-sulfur batteries, and performance tests were performed. The test results are shown in Table 1.
[0050] Test method: First, set the discharge current at different rates (0.1C, 0.5C, 2C) to charge the battery at constant current until the voltage reaches the set maximum value, then switch to constant voltage charging until the current drops to the set minimum value. Next, perform a constant current discharge test until the battery voltage drops to the set minimum value. Test the first discharge capacity at 0.1C rate.
[0051] Table 1 Test results
[0052] As shown in Table 1, Example 1 is superior to other examples and comparative examples in multiple key performance indicators. The reasons can be attributed to the following points: appropriate Cu-Ni ratio, the mass ratio of Cu and Ni used in Example 1 is 1:1, this ratio provides the best synergistic effect in Cu-Ni / MOF nanoparticles, Cu and Ni can more effectively catalyze the adsorption and conversion of polysulfides under the joint action, reduce the dissolution and loss of polysulfides in the electrolyte, thereby improving the cycle stability and capacity retention rate of the battery; suitable MOF structure, MOF (Metal-Organic Frameworks) has a highly ordered pore structure, which can effectively capture polysulfides and prevent them from migrating to the negative electrode. The Cu-Ni / MOF nanoparticles in Example 1 form a uniform and stable covering layer on the polyacrylonitrile nanofiber matrix, and this structure ensures the efficient capture and conversion of polysulfides. Precise electrospinning process, Example 1 uses optimized parameters such as 12% polyacrylonitrile solution concentration, 18KV spray voltage and 120-140mm receiving distance, which ensure the uniform distribution of nanofibers and suitable pore structure, so that the electrolyte can be better penetrated and retained, which helps to improve ion conductivity and thus improve the overall performance of the battery; moderate thickness ratio, the thickness ratio of Cu-Ni / MOF nanoparticles to polyacrylonitrile nanofiber matrix in Example 1 ensures that the nanoparticles have sufficient coverage on the matrix, while not hindering ion migration due to excessive coverage, and this moderate thickness ratio helps to achieve the best electrochemical performance. The above data show that the synergistic effect of Cu-Ni / MOF nanoparticles, the effective use of porous structures and the precise control of electrospinning parameters are all the keys to its success. These factors work together to enable lithium-sulfur batteries to have high first discharge capacity, excellent cycle stability and capacity retention at high rates.
[0053] The materials in this embodiment 1 were identified, wherein: Figure 1 (a) is the TEM image of Cu-Ni / MOF nanoparticles; Figure 1 b is the element mapping diagram of Cu-Ni / MOF nanoparticles; Figure 1 c- Figure 1 g is the distribution diagram of C, N, O, Cu, and Ni elements in Cu-Ni / MOF nanoparticles, indicating that each element is evenly distributed; Figure 1 (h) is PAN nanofiber; Figure 1 (i) is the surface micromorphology of the composite membrane coating layer; Figure 1 (j) is a cross-sectional microscopic morphology of the composite diaphragm, showing the thickness of the coating layer and the nanofiber layer.
[0054] The present application coats diatomic Cu-Ni / MOF nanoparticles on the surface of a polyacrylonitrile nanofiber substrate so that the diatomic Cu-Ni / MOF nanoparticles are evenly distributed on the surface of the polyacrylonitrile nanofiber substrate, which is beneficial to the improvement of the sites and spaces for capturing and converting polysulfides by the composite modified diaphragm of the lithium-sulfur battery, and the efficiency of capturing and converting polysulfides is enhanced to reduce the shuttling effect of polysulfides, and ultimately improve the coulombic efficiency, capacity retention rate and cycle stability of the lithium-sulfur battery.
[0055] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A lithium-sulfur battery composite modified diaphragm, characterized in that: The invention comprises a polyacrylonitrile nanofiber matrix and Cu-Ni / MOF nanoparticles coated on the surface of the polyacrylonitrile nanofiber matrix.
2. The lithium-sulfur battery composite modified diaphragm according to claim 1, characterized in that: The porosity of the polyacrylonitrile nanofiber matrix is 60-65%, and the average pore diameter of the polyacrylonitrile nanofiber matrix is 20-25 nm.
3. A method for preparing a composite modified diaphragm for a lithium-sulfur battery as claimed in claim 1, characterized in that: The following steps are involved: S1. Obtaining Cu-Ni / MOF nanoparticles; S2. Using polyacrylonitrile solution as raw material, preparing polyacrylonitrile nanofiber matrix by electrospinning process; S3. dispersing the Cu-Ni / MOF nanoparticles in a solvent, and then coating the Cu-Ni / MOF nanoparticles on the surface of the polyacrylonitrile nanofiber substrate to obtain a nanofiber membrane; S4. Drying the nanofiber membrane to obtain the lithium-sulfur battery composite modified membrane.
4. The method for preparing a composite modified diaphragm for a lithium-sulfur battery according to claim 3, characterized in that: In step S1, the preparation method of Cu-Ni / MOF nanoparticles is: adding Ni(NO3)2·6H2O and Cu(NO3)2·3H2O to a mixture of anhydrous ethanol, pure water and DMF to obtain an intermediate product, then adding BTC to the intermediate product, heating to react, filtering, washing and drying the precipitate to obtain Cu-Ni / MOF nanoparticles.
5. The method for preparing a composite modified diaphragm for a lithium-sulfur battery according to claim 4, characterized in that: The volume ratio of the anhydrous ethanol, pure water and DMF is 1:1:1-2.
6. The method for preparing a composite modified diaphragm for a lithium-sulfur battery according to claim 4, characterized in that: The mass ratio of Ni(NO3)2·6H2O to Cu(NO3)2·3H2O is 1:1-2.
7. The method for preparing a composite modified diaphragm for a lithium-sulfur battery according to claim 4, characterized in that: The heating reaction temperature is 160-170° C., and the heating reaction time is 4-8 hours.
8. The method for preparing a composite modified diaphragm for a lithium-sulfur battery according to claim 3, characterized in that: In step S3, the thickness ratio of the Cu-Ni / MOF nanoparticles to the polyacrylonitrile nanofiber matrix is 0.1-1:
2.
9. The method for preparing a composite modified diaphragm for a lithium-sulfur battery according to claim 3, characterized in that: The process conditions of the electrospinning are: solution concentration 10-15%, spray voltage 18-20KV, receiving distance 120-140mm, solution propulsion speed 0.025-0.03ml / min, and needle diameter 0.8-0.9mm.
10. A lithium-sulfur battery, characterized in that: It comprises a lithium-sulfur battery composite modified diaphragm obtained by the preparation method according to any one of claims 2 to 9.
Citation Information
Cited By
Copper-doped bismuth telluride topological insulator lithium-sulfur battery diaphragm material and preparation method thereof
CN121341956A