Organic ultraviolet photoelectric detector and preparation method and related equipment thereof
By using wide-bandgap p-type and n-type organic semiconductor heterojunction photosensitive layers in organic ultraviolet photodetectors, the problems of high dark current and low sensitivity are solved, and the effect of efficient ultraviolet light detection and significant suppression of dark current is achieved. .
Patent Information
- Application Number
- CN202310620509.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
Existing organic ultraviolet photodetectors have problems with excessive dark current and low sensitivity.
The bulk heterojunction photosensitive layer is adopted, including at least one p-type organic semiconductor and an n-type organic semiconductor, to ensure that its bandwidth is greater than or equal to 3.2 eV, and to maintain the highest molecular energy level and n-type of the p-type organic semiconductor. The difference in the lowest unoccupied molecular energy level of an organic semiconductor is greater than or equal to 1.3 eV, and the barrier between the anode or cathode and the bulk heterojunction photosensitive layer is greater than or equal to 2 eV, to prevent heterocharge injection.
Efficient detection of visible blind ultraviolet or sun-blind ultraviolet light is achieved, which significantly reduces the dark current, ensures high light current while suppressing dark current, making it less than 1nA/cm2, and improves the UV/visible suppression ratio greater than 104.
Smart Images

Figure CN119053158A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optoelectronic devices, and in particular to an organic ultraviolet photodetector and a preparation method and related equipment thereof. Background Art
[0002] UV photodetectors have many important applications, such as monitoring the UV index of sunlight to prevent UV damage to the human body, and can also be used to detect UV curing, UV chemical reactions, UV water purification and air disinfection, UV germicidal lamps, and fire alarms. In the military, UV photodetectors can be used for UV communications, UV guidance, etc. At present, commercial UV photodetectors are mainly based on inorganic semiconductors such as GaN and SiC. Their preparation process is extremely complex, the cost is very high, and they are not environmentally friendly. The growth of detector crystal materials has strict requirements on the lattice matching of substrate materials, and their growth environment is difficult to control and consumes high energy, resulting in high costs. In comparison, organic UV photodetectors with organic photodiodes as functional devices have gradually received widespread attention due to their many advantages such as high sensitivity, good flexibility, light weight, simple preparation process, low cost, and environmental protection. However, progress in the field of organic UV photodetectors is very slow, and existing organic UV photodetectors have problems such as high dark current and low sensitivity.
[0003] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide an organic ultraviolet photodetector and a preparation method and related equipment thereof, aiming to solve the problem of excessively high dark current in the existing organic ultraviolet photodetectors.
[0005] The technical solution of the present invention is as follows:
[0006] In a first aspect of the present invention, an organic ultraviolet photodetector is provided, comprising an anode, a cathode and a bulk heterojunction photosensitive layer disposed between the anode and the cathode, wherein the potential barrier between the anode and the bulk heterojunction photosensitive layer and the potential barrier between the cathode and the bulk heterojunction photosensitive layer are both greater than or equal to 2 eV;
[0007] The bulk heterojunction photosensitive layer comprises at least one p-type organic semiconductor and at least one n-type organic semiconductor, and the band gaps of the p-type organic semiconductor and the n-type organic semiconductor are both greater than or equal to 3.2 eV;
[0008] The difference between the highest occupied molecular energy level of the p-type organic semiconductor and the lowest unoccupied molecular energy level of the n-type organic semiconductor is greater than or equal to 1.3 eV.
[0009] The second aspect of the present invention provides a method for preparing the organic ultraviolet photodetector as described above, which comprises the steps of:
[0010] providing an anode;
[0011] forming a bulk heterojunction photosensitive layer on the anode;
[0012] forming a cathode on the bulk heterojunction photosensitive layer to obtain the organic ultraviolet photodetector;
[0013] or, providing a cathode;
[0014] forming a bulk heterojunction photosensitive layer on the cathode;
[0015] An anode is formed on the bulk heterojunction photosensitive layer to obtain the organic ultraviolet photodetector.
[0016] According to a third aspect of the present invention, there is provided an ultraviolet image sensor, which includes the organic ultraviolet photoelectric sensor as described above.
[0017] A fourth aspect of the present invention provides an electronic device, which includes the ultraviolet image sensor described above.
[0018] Beneficial effect: The p-type organic semiconductor and the n-type organic semiconductor in the bulk heterojunction photosensitive layer of the present invention both have wide band gaps, and the band gap widths are both greater than or equal to 3.2 eV, so light detection in the visible-blind ultraviolet band (wavelength < 400 nm) or day-blind ultraviolet band (wavelength < 300 nm) can be achieved, and the ultraviolet / visible suppression ratio is greater than 10 4 Since both p-type organic semiconductors and n-type organic semiconductors have wide band gaps, the dark current caused by thermal excitation can be almost ignored. At this time, the main source of the dark current is the injection of electrons and holes from the anode and cathode respectively under reverse bias. Therefore, in the present invention, the difference between the highest occupied molecular energy level of the p-type organic semiconductor and the lowest unoccupied molecular energy level of the n-type organic semiconductor is maintained at an energy level difference greater than or equal to 1.3 eV, and the potential barrier between the anode or cathode and the bulk heterojunction photosensitive layer is greater than or equal to 2 eV, which effectively blocks the injection of hetero charges in the dark state, ensures high photocurrent and effectively suppresses the dark current, making the dark current less than 1 nA / cm 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the structure of an organic ultraviolet photodetector in an embodiment of the present invention.
[0020] Figure 2 Schematic diagram of the structure of the encapsulated organic ultraviolet photodetector in an embodiment of the present invention.
[0021] Figure 3 A schematic diagram of the energy levels of the organic ultraviolet photodetector provided in Example 1 of the present invention.
[0022] Figure 4 A schematic diagram of the energy levels of the organic ultraviolet photodetector provided in Example 2 of the present invention.
[0023] Figure 5 This is the UV-visible absorption spectrum of the bulk heterojunction photosensitive layer material used in Example 14 of the present invention.
[0024] Figure 6 This is the light response spectrum of the organic ultraviolet photodetector in Example 14 of the present invention. DETAILED DESCRIPTION
[0025] The present invention provides an organic ultraviolet photodetector and a preparation method thereof and related equipment. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0027] The present invention does not limit the specific structure of the organic ultraviolet photodetector, which can be a positive structure or a reverse structure. Figure 1 Taking the inversion structure shown in the figure as an example, an embodiment of the present invention provides an organic ultraviolet photodetector, which includes an anode 106, a cathode 102, and a bulk heterojunction photosensitive layer 104 arranged between the anode 106 and the cathode 102, and the potential barrier between the anode 106 and the bulk heterojunction photosensitive layer 104 and the potential barrier between the cathode 102 and the bulk heterojunction photosensitive layer 104 are both greater than or equal to 2eV;
[0028] The bulk heterojunction photosensitive layer comprises at least one p-type organic semiconductor and at least one n-type organic semiconductor, and the band gaps of the p-type organic semiconductor and the n-type organic semiconductor are both greater than or equal to 3.2 eV;
[0029] The difference between the highest occupied molecular energy level of the p-type organic semiconductor and the lowest unoccupied molecular energy level of the n-type organic semiconductor is greater than or equal to 1.3 eV (the difference is taken as an absolute value).
[0030] In the embodiment of the present invention, the potential barrier between the anode and the bulk heterojunction photosensitive layer is the energy level difference between the lowest unoccupied molecular energy level of the p-type organic semiconductor and the work function of the anode, and the potential barrier between the cathode and the bulk heterojunction photosensitive layer is the energy level difference between the highest occupied molecular energy level of the n-type organic semiconductor and the work function of the cathode.
[0031] In the bulk heterojunction photosensitive layer of the embodiment of the present invention, both the p-type organic semiconductor and the n-type organic semiconductor have wide band gaps, and the band gap width is greater than or equal to 3.2 eV, so that light detection in the visible blind ultraviolet band (wavelength < 400nm) or solar blind ultraviolet band (wavelength < 300nm) can be achieved, and the ultraviolet / visible suppression ratio is greater than 10 4 Since both p-type organic semiconductors and n-type organic semiconductors have wide band gaps, the dark current caused by thermal excitation can be almost ignored. At this time, the main source of the dark current is the electrons and holes injected from the cathode and anode respectively under reverse bias. Therefore, in the present invention, the difference between the highest occupied molecular energy level of the p-type organic semiconductor and the lowest unoccupied molecular energy level of the n-type organic semiconductor is maintained at an energy level difference greater than or equal to 1.3 eV, and the potential barrier between the anode or cathode and the bulk heterojunction photosensitive layer is greater than or equal to 2 eV, which can ensure that there is sufficient electron and hole injection barrier under reverse bias, effectively block hetero charge injection in the dark state, ensure high photocurrent and effectively suppress dark current, so that the dark current is less than 1 nA / cm 2 .
[0032] In some embodiments, the highest molecular occupied energy level of the p-type organic semiconductor is -4.9 to -6.0 eV, and the lowest molecular unoccupied energy level of the n-type organic semiconductor is -1.1 to -4.5 eV.
[0033] In some embodiments, in the bulk heterojunction photosensitive layer, the mass ratio of the p-type organic semiconductor to the n-type organic semiconductor is 3:1 to 1:3.
[0034] In some embodiments, Figure 1 As shown, the organic ultraviolet photodetector further includes a hole transport layer 105 or an electron blocking layer 105 disposed between the anode 106 and the bulk heterojunction photosensitive layer 104, and the material of the hole transport layer or the electron blocking layer is a p-type semiconductor material. In some specific embodiments, the p-type semiconductor material can be a p-type organic semiconductor in the bulk heterojunction photosensitive layer.
[0035] In some embodiments, Figure 1As shown, the organic ultraviolet photodetector further includes an electron transport layer 103 or a hole blocking layer 103 disposed between the cathode 102 and the bulk heterojunction photosensitive layer 104, and the material of the electron transport layer or the hole blocking layer is an n-type semiconductor material.
[0036] In some specific embodiments, the n-type semiconductor may be an n-type organic semiconductor in a bulk heterojunction photosensitive layer.
[0037] In some embodiments, at least one of the anode and the cathode is a transparent electrode, and the transmittance of the transparent electrode to the ultraviolet band is greater than 80%.
[0038] In some embodiments, the transparent electrode includes at least one of an indium tin oxide (ITO) electrode, a fluorine-doped tin oxide (FTO) electrode, a silver nanowire electrode, and a thin-layer metal electrode with a thickness ranging from 2 to 20 nm.
[0039] In some embodiments, the material of the thin metal electrode includes but is not limited to at least one of gold, platinum, silver, copper, aluminum, calcium, nickel, chromium, and titanium. For example, the thin metal electrode may be a thin metal electrode in which a gold layer and a platinum layer are stacked, a thin metal electrode in which a silver layer and a copper layer are stacked, etc.
[0040] In some embodiments, Figure 1 As shown, the organic ultraviolet photodetector further includes a substrate 101 , which is disposed on a side of the cathode 102 away from the bulk heterojunction photosensitive layer 104 or on a side of the anode 106 away from the bulk heterojunction photosensitive layer 104 . Figure 1 In the figure, it is taken as an example that the substrate 101 is disposed on a side of the cathode 102 away from the bulk heterojunction photosensitive layer 104 .
[0041] In some embodiments, the substrate is a rigid substrate or a flexible substrate, the rigid substrate includes but is not limited to at least one of glass (such as ordinary glass, quartz glass), silicon wafer, and sapphire, and the flexible substrate includes but is not limited to at least one of polyethylene, polymethyl methacrylate, polycarbonate, polyurethane, polyimide, chloroacetic acid resin, and polyacrylic acid.
[0042] In some embodiments, the organic ultraviolet photodetector provided by the embodiment of the present invention may be packaged, and the structure after packaging is as follows: Figure 2As shown. That is, the packaged organic ultraviolet photodetector includes an organic ultraviolet photodetector, a metal plate 107 connecting the cathode 102 and the anode 106 of the organic ultraviolet photodetector, and an insulating layer 108 which is partially arranged on the outer surface of the organic ultraviolet photodetector and partially arranged between the organic ultraviolet photodetector and the metal plate (that is, the insulating layer is divided into two parts, one part is arranged on the outer surface of the organic ultraviolet photodetector, and the other part is arranged between the organic ultraviolet photodetector and the metal plate).
[0043] In some embodiments, the p-type organic semiconductor is a small molecule organic semiconductor material. Specifically, the p-type organic semiconductor is selected from at least one of the following structures:
[0044]
[0045]
[0046]
[0047]
[0048]
[0049]
[0050]
[0051]
[0052]
[0053]
[0054] In some embodiments, the n-type organic semiconductor is a small molecule organic semiconductor material. Specifically, the n-type organic semiconductor is selected from one of the following structures:
[0055]
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063]
[0064]
[0065] These p-type and n-type organic small molecule semiconductors have a relatively strong π-π stacking structure, good coplanarity, and high carrier mobility; at the same time, the introduction of some special functional groups such as halogen atoms will also enhance the electron-withdrawing ability of the overall molecule.
[0066] The present invention also provides a method for preparing the organic ultraviolet photodetector as described above in the present invention, which comprises the steps of:
[0067] S11, providing an anode;
[0068] S12, forming a bulk heterojunction photosensitive layer on the anode;
[0069] S13, forming a cathode on the bulk heterojunction photosensitive layer to obtain the organic ultraviolet photodetector.
[0070] The embodiment of the present invention also provides another method for preparing the organic ultraviolet photodetector as described above in the embodiment of the present invention, which comprises the steps of:
[0071] S21, providing a cathode;
[0072] S22, forming a bulk heterojunction photosensitive layer on the cathode;
[0073] S23, forming an anode on the bulk heterojunction photosensitive layer to obtain the organic ultraviolet photodetector.
[0074] In this embodiment, the materials and energy level relationships of the anode, cathode and bulk heterojunction photosensitive layer can be found in the above description and will not be repeated here.
[0075] In step S12, in some embodiments, a bulk heterojunction photosensitive layer is formed on the anode by evaporation. Specifically, at least one p-type organic semiconductor and at least one n-type organic semiconductor are co-evaporated on the anode by evaporation, and the ratio of the two is regulated by controlling the evaporation rates of the two, so as to form a bulk heterojunction photosensitive layer on the anode.
[0076] In step S22, in some embodiments, a bulk heterojunction photosensitive layer is formed on the cathode by evaporation. Specifically, at least one p-type organic semiconductor and at least one n-type organic semiconductor are co-evaporated on the cathode by evaporation, and the ratio of the two is regulated by controlling the evaporation rates of the two, so as to form a bulk heterojunction photosensitive layer on the cathode.
[0077] In this embodiment, the concentration of the donor (n-type organic semiconductor) and acceptor (p-type organic semiconductor) molecules in the bulk heterojunction photosensitive layer is precisely controlled by the evaporation rate, so that the stability and repeatability of the film quality can be ensured, as well as the compatibility with the current detector manufacturing and chip integration processes. Furthermore, the evaporation process is more suitable when both the p-type organic semiconductor and the n-type organic semiconductor are organic small molecule materials.
[0078] An embodiment of the present invention further provides an ultraviolet image sensor, which includes the organic ultraviolet photodetector described above in the embodiment of the present invention.
[0079] An embodiment of the present invention further provides an electronic device, which includes the ultraviolet image sensor described above in the embodiment of the present invention.
[0080] The following describes it in detail through specific embodiments.
[0081] Example 1
[0082] The present embodiment provides an organic ultraviolet photodetector, including a quartz glass substrate, an ITO conductive cathode, an NDI-C6 electron transport layer, a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and NDI-C6 of 1:1, a C8-BTBT hole transport layer, and an Ag conductive anode, which are stacked in sequence from bottom to top.
[0083] Among them, the structural formula of C8-BTBT is:
[0084] Its bandgap is 3.4eV;
[0085] The structural formula of NDI-C6 is: Its bandgap is 3.2eV;
[0086] The difference between the highest occupied molecular energy level of C8-BTBT (−5.6 eV) and the lowest unoccupied molecular energy level of NDI-C6 (−3.8 eV) is 1.8 eV;
[0087] The energy level difference between the lowest unoccupied molecular energy level of C8-BTBT and the work function of the Ag conductive anode is 2.4 eV;
[0088] The energy level difference between the highest occupied molecular energy level of NDI-C6 and the work function of the ITO conductive cathode is 2.5 eV.
[0089] The method for preparing the organic ultraviolet photodetector comprises the steps of:
[0090] (1) Cleaning the substrate composed of a quartz glass substrate and an ITO conductive cathode, and drying it with nitrogen after cleaning;
[0091] (2) treating the cleaned substrate with UV / ozone for 15 min;
[0092] (3) vapor-depositing a 10 nm thick NDI-C6 film on the ITO conductive cathode of the treated substrate to form an NDI-C6 electron transport layer;
[0093] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1 on the surface of the NDI-C6 electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0094] (5) evaporating a 10 nm thick C8-BTBT film on the bulk heterojunction photosensitive layer to form a C8-BTBT hole transport layer;
[0095] (6) After annealing at 80° C. for 10 minutes in a glove box, a 100 nm thick Ag conductive anode was evaporated on the C8-BTBT hole transport layer through a mask to obtain an organic ultraviolet photodetector.
[0096] The device was tested in air: at -2V bias, the dark current of the device was 1.5×10 -9 A / cm 2 ; The device's responsivity was measured to be 0.168A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate; the device's responsivity was measured to be 0.112A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; the device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0097] The energy level diagram of the organic ultraviolet photodetector provided in this embodiment is as follows Figure 3 As shown, 101 is a quartz glass substrate, 102 is an ITO conductive cathode, 103 is an NDI-C6 electron transport layer, 104 is a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and NDI-C6 of 1:1, 105 is a C8-BTBT hole transport layer, and 106 is an Ag conductive anode.
[0098] Example 2
[0099] The present embodiment provides an organic ultraviolet photodetector, including a quartz glass substrate, an ITO conductive anode, a PEDOT:PSS hole transport layer, a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and NDI-C6 of 1:1, an NDI-C6 electron transport layer, and an Al conductive cathode, which are stacked in sequence from bottom to top.
[0100] Among them, the energy level difference between the lowest unoccupied molecular energy level of C8-BTBT and the work function of the ITO conductive anode is 2.8 eV;
[0101] The energy level difference between the highest occupied molecular energy level of NDI-C6 and the work function of the Al conductive cathode is 2.8 eV.
[0102] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0103] (1) Cleaning the substrate composed of a quartz glass substrate and an ITO conductive anode, and drying it with nitrogen after cleaning;
[0104] (2) treating the cleaned substrate with UV / ozone for 15 min;
[0105] (3) spin coating a 10 nm thick PEDOT:PSS hole transport layer on the ITO conductive anode of the treated substrate and annealing at 150 °C in air for 10 min;
[0106] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1 on the PEDOT:PSS hole transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0107] (5) vapor depositing a 10 nm thick NDI-C6 thin film on the bulk heterojunction photosensitive layer to form an NDI-C6 electron transport layer;
[0108] (6) After annealing at 80° C. for 10 minutes in a glove box, a 100 nm thick Al conductive cathode was evaporated on the NDI-C6 electron transport layer through a mask to obtain an organic ultraviolet photodetector.
[0109] The device was tested in air: at -2 V bias, the dark current of the device was 3.2 × 10 -9 A / cm 2 ; The device's responsivity was measured to be 0.148A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate, and 0.092A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; The device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0110] The energy level diagram of the organic ultraviolet photodetector provided in this embodiment is as follows Figure 4As shown, 101 is a quartz glass substrate, 102 is an ITO conductive anode, 103 is a PEDOT:PSS hole transport layer, 104 is a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and NDI-C6 of 1:1, 105 is an NDI-C6 electron transport layer, and 106 is an Al conductive cathode.
[0111] Example 3
[0112] This embodiment provides an organic ultraviolet photodetector, which is basically the same as the organic ultraviolet photodetector in Embodiment 1, except that the electron transport layer is a SnO2 electron transport layer and the hole transport layer is a MoO3 hole transport layer.
[0113] Among them, the band gap width of SnO2 is 3.8eV, and the band gap width of MoO3 is 3.55eV.
[0114] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0115] (1) The same as step (1) in Example 1;
[0116] (2) The same as step (2) in Example 1;
[0117] (3) Spin-coating a 10 nm thick SnO2 film on the ITO conductive cathode of the treated substrate and annealing it in air at 150°C for 10 minutes to form a SnO2 electron transport layer;
[0118] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1 on the SnO2 electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0119] (5) vapor depositing a 10 nm thick MoO3 thin film on the bulk heterojunction photosensitive layer to form a MoO3 hole transport layer;
[0120] (6) After annealing at 80° C. for 10 minutes in a glove box, a 100 nm thick Ag conductive anode was evaporated on the MoO 3 hole transport layer through a mask to obtain an organic ultraviolet photodetector.
[0121] The device was tested in air: at -2 V bias, the dark current of the device was 2.8 × 10 -9 A / cm 2; The device's responsivity was measured to be 0.168A / W under 365nm ultraviolet light from the bottom quartz glass substrate, and the device's responsivity was measured to be 0.11A / W under 254nm ultraviolet light from the bottom quartz glass substrate; the device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0122] Example 4
[0123] This embodiment provides an organic ultraviolet photodetector, which is basically the same as the organic ultraviolet photodetector in Embodiment 1, except that the electron transport layer is a PEIE electron transport layer.
[0124] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0125] (1) The same as step (1) in Example 1;
[0126] (2) The same as step (2) in Example 1;
[0127] (3) spin coating a 10 nm thick PEIE film on the ITO conductive cathode of the treated substrate, and annealing at 150° C. in air for 10 min to form a PEIE electron transport layer;
[0128] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1 on the PEIE electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0129] (5) The same as step (5) in Example 1;
[0130] (6) Same as step (6) in Example 1.
[0131] The device was tested in air: at -2 V bias, the dark current of the device was 1.2 × 10 -9 A / cm 2 The device's responsivity is 0.169A / W when the 365nm ultraviolet light is irradiated from the bottom quartz glass substrate, and the responsivity is 0.115A / W when the 254nm ultraviolet light is irradiated from the bottom quartz glass substrate; the device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0132] Example 5
[0133] This embodiment provides an organic ultraviolet photodetector, which is basically the same as the organic ultraviolet photodetector in Example 4, except that the hole transport layer is a MoO3 hole transport layer.
[0134] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0135] (1)-(4) are the same as steps (1)-(4) in Example 4.
[0136] (5) a MoO3 thin film with a thickness of 10 nm is evaporated on the bulk heterojunction photosensitive layer to form a MoO3 hole transport layer;
[0137] (6) After annealing at 80° C. for 10 minutes in a glove box, a 100 nm thick Ag conductive anode was evaporated on the MoO 3 hole transport layer through a mask to obtain an organic ultraviolet photoelectric device.
[0138] The device was tested in air: at -2 V bias, the dark current of the device was 1.2 × 10 -9 A / cm 2 ; The device's responsivity was measured to be 0.168A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate, and 0.116A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; The device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0139] Example 6
[0140] This embodiment provides an organic ultraviolet photodetector, which is basically the same as the organic ultraviolet photodetector in Example 5, except that the bulk heterojunction photosensitive layer is a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and NDI-C6 of 1.5:1.
[0141] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0142] (1)-(3) are the same as steps (1)-(3) in Example 5;
[0143] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1.5:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1.5:1 on the PEIE electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0144] (5)-(6) are the same as steps (5)-(6) in Example 5.
[0145] The device was tested in air: at -2 V bias, the dark current of the device was 1.2 × 10 -9 A / cm 2; The device's responsivity was measured to be 0.132A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate, and 0.085A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; The device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0146] Example 7
[0147] This embodiment provides an organic ultraviolet photodetector, which is basically the same as the organic ultraviolet photodetector in Example 5, except that the bulk heterojunction photosensitive layer is a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and NDI-C6 of 1:1.5.
[0148] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0149] (1)-(3): the same as steps (1)-(3) in Example 5;
[0150] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1.5, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1.5 on the PEIE electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0151] (5)-(6) are the same as steps (5)-(6) in Example 5.
[0152] The device was tested in air: at -2 V bias, the dark current of the device was 8.6 × 10 -10 A / cm 2 The device's responsivity is 0.136A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate, and 0.091A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; the device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0153] Example 8
[0154] The present embodiment provides an organic ultraviolet photodetector, comprising a silicon wafer substrate, a thin layer of Cr / Ag conductive cathode, a PEIE electron transport layer, a bulk heterojunction photosensitive layer with a C8-BTBT and NDI-C6 ratio of 1:1, a MoO3 hole transport layer, and an Ag conductive anode stacked in sequence from bottom to top.
[0155] Among them, the energy level difference between the lowest unoccupied molecular energy level of C8-BTBT and the work function of the Ag conductive anode is 2.4 eV;
[0156] The energy level difference between the highest occupied molecular energy level of NDI-C6 and the work function of the thin-layer Cr / Ag conductive cathode is 2.5 eV.
[0157] The device preparation process of the above-mentioned organic ultraviolet photodetector includes the following steps:
[0158] (1) Cleaning the silicon wafer substrate and drying it with nitrogen gas after cleaning;
[0159] (2) depositing a 5 nm thick Cr layer and a 40 nm thick Ag layer on the cleaned silicon wafer substrate in sequence, with the shapes determined by a mask plate, to form a thin layer Cr / Ag conductive cathode;
[0160] (3) spin coating a 5 nm thick PEIE film on the Ag layer of the thin Cr / Ag conductive cathode and annealing at 100 °C in air for 10 min to form a PEIE electron transport layer;
[0161] (4) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1 on the PEIE electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 200 nm;
[0162] (5) vapor depositing a 10 nm thick MoO3 thin film on the bulk heterojunction photosensitive layer to form a MoO3 hole transport layer;
[0163] (6) Annealing at 80° C. for 10 minutes in a glove box; and evaporating a 10 nm thick Ag conductive anode layer on the MoO3 hole transport layer through a mask.
[0164] The device was tested in air: at -2 V bias, the dark current of the device was 2.1×10 -9 A / cm 2 The device responsivity was measured to be 0.186A / W when irradiated with 365nm UV light from the top Ag conductive anode, and 0.124A / W when irradiated with 254nm UV light from the top Ag conductive anode. The response band was 200-375nm, and the UV / visible suppression ratio was greater than 10. 4 .
[0165] Example 9
[0166] This embodiment provides an organic ultraviolet photodetector and a method for preparing the same, which is different from Embodiment 5 only in that the thickness of the bulk heterojunction photosensitive layer is 300 nm.
[0167] The device was tested in air: at -2 V bias, the dark current of the device was 5.6 × 10 -10 A / cm 2The device responsivity is 0.172A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate; the device responsivity is 0.122A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate. The response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0168] Example 10
[0169] This embodiment provides an organic ultraviolet photodetector and a preparation method thereof, which is different from Embodiment 1 only in that the thickness of the bulk heterojunction photosensitive layer is 300 nm, and the thickness of the Ag conductive anode is 10 nm.
[0170] The device was tested in air: at -2 V bias, the dark current of the device was 4.9 × 10 -10 A / cm 2 The device responsivity was measured to be 0.198A / W when irradiated with 365nm UV light from the top Ag conductive anode, and 0.138A / W when irradiated with 254nm UV light from the top Ag conductive anode. The response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0171] Embodiment 11
[0172] The present embodiment provides an organic ultraviolet photodetector, including a quartz glass substrate, an ITO conductive cathode, an NDI-C6 electron transport layer, a bulk heterojunction photosensitive layer with a mass ratio of C12-Ph-BTBT and NDI-C6 of 1:1, a MoO3 hole transport layer, and an Ag conductive anode 106, which are stacked in sequence from bottom to top.
[0173] Among them, the structure of C12-Ph-BTBT is Its bandgap is 3.15eV;
[0174] The difference between the highest occupied molecular energy level of C12-Ph-BTBT (-5.5 eV) and the lowest unoccupied molecular energy level of NDI-C6 (-3.8 eV) is 1.7 eV;
[0175] The energy level difference between the lowest unoccupied molecular energy level of C12-Ph-BTBT and the work function of the Ag conductive anode is 2.3 eV.
[0176] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0177] (1) Cleaning the substrate composed of a quartz glass substrate and an ITO conductive cathode, and drying it with nitrogen after cleaning;
[0178] (2) treating the cleaned substrate with UV / ozone for 15 minutes;
[0179] (3) vapor-depositing a 10 nm thick NDI-C6 film on the ITO conductive cathode of the treated substrate to form an NDI-C6 electron transport layer;
[0180] (4) controlling the evaporation rate of C12-Ph-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C12-Ph-BTBT and NDI-C6 of 1:1 on the NDI-C6 electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 300 nnm;
[0181] (5) vapor depositing a 10 nm thick MoO3 thin film on the surface of the bulk heterojunction photosensitive layer to form a MoO3 hole transport layer;
[0182] (6) After annealing at 80° C. for 10 minutes in a glove box, a 10 nm thick Ag conductive anode layer was evaporated on the MoO 3 hole transport layer through a mask.
[0183] The device was tested in air: at -2 V bias, the dark current of the device was 6.5 × 10 -10 A / cm 2 ; The device's responsivity was measured to be 0.176A / W when irradiated with 365nm ultraviolet light from the top Ag conductive anode, and 0.119A / W when irradiated with 254nm ultraviolet light; The device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 3 .
[0184] Example 12
[0185] The present embodiment provides an organic ultraviolet photodetector, including a quartz glass substrate, an ITO conductive cathode, an NDI-C6 electron transport layer, a bulk heterojunction photosensitive layer with a mass ratio of Ph-BTBT and NDI-C6 of 1:1, a C8-BTBT hole transport layer, and an Ag conductive anode, which are stacked in sequence from bottom to top.
[0186] Among them, the structural formula of Ph-BTBT is Its bandgap is 3.43eV;
[0187] The difference between the highest occupied molecular energy level of Ph-BTBT (−5.6 eV) and the lowest unoccupied molecular energy level of NDI-C6 (−3.8 eV) is 1.8 eV;
[0188] The energy level difference between the lowest unoccupied molecular energy level of Ph-BTBT and the work function of the Ag conductive anode is 2.45 eV.
[0189] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0190] (1) Cleaning the substrate composed of a quartz glass substrate and an ITO conductive cathode, and drying it with nitrogen after cleaning;
[0191] (2) UV / Ozone treatment of the cleaned substrate for 15 minutes;
[0192] (3) vapor-depositing a 10 nm thick NDI-C6 film on the ITO conductive cathode of the treated substrate to form an NDI-C6 electron transport layer;
[0193] (4) controlling the evaporation rate of Ph-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of Ph-BTBT and NDI-C6 of 1:1 on the NDI-C6 electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 300 nm;
[0194] (5) evaporating a 10 nm thick C8-BTBT film on the surface of the bulk heterojunction photosensitive layer to form a C8-BTBT hole transport layer;
[0195] (6) Annealing treatment was performed at 80° C. for 10 minutes in a glove box, and a 10 nm thick Ag conductive anode was evaporated on the C8-BTBT hole transport layer through a mask to obtain an organic ultraviolet photodetector.
[0196] The device was tested in air: at -2V bias, the dark current was 6.9×10 -10 A / cm 2 ; The device's responsivity was measured to be 0.181A / W when irradiated with 365nm UV light from the top Ag conductive anode, and 0.115A / W when irradiated with 254nm UV light from the top Ag conductive anode; The device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0197] Example 13
[0198] This embodiment provides an organic ultraviolet photodetector, which is different from Embodiment 1 only in that the cathode is a thin layer of Cr / Ag conductive cathode, the thickness of the bulk heterojunction photosensitive layer is 300nm, and the thickness of the Ag conductive anode is 10nm.
[0199] The energy level difference between the highest occupied molecular energy level of NDI-C6 and the work function of the thin-layer Cr / Ag conductive cathode is 2.5 eV.
[0200] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0201] (1) Cleaning the quartz glass substrate and drying it with nitrogen gas;
[0202] (2) a chromium layer with a thickness of 2 nm and a silver layer with a thickness of 5 nm were sequentially deposited on a cleaned quartz glass substrate to form a thin-layer Cr / Ag cathode;
[0203] (3) treating the quartz glass substrate with the above-mentioned evaporated electrode with UV / ozone for 15 minutes;
[0204] (4) evaporating a 10 nm thick NDI-C6 film on the Ag layer of the thin-layer Cr / Ag conductive cathode to form an NDI-C6 electron transport layer;
[0205] (5) controlling the evaporation rate of C8-BTBT and NDI-C6 to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and NDI-C6 of 1:1 on the NDI-C6 electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 300 nm;
[0206] (6) vapor-depositing a 10 nm thick C8-BTBT film on the bulk heterojunction photosensitive layer to form a C8-BTBT hole transport layer;
[0207] (7) After annealing at 80° C. for 10 minutes in a glove box, a 10 nm thick Ag conductive anode was evaporated on the C8-BTBT hole transport layer through a mask.
[0208] The device was tested in air: at -2 V bias, the dark current of the device was 4.9 × 10 -10 A / cm 2 ; The device's responsivity was measured to be 0.208A / W when irradiated with 365nm ultraviolet light from the bottom quartz glass substrate, and 0.145A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; The device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0209] Embodiment 14
[0210] The present embodiment provides an organic ultraviolet photodetector, comprising a quartz glass substrate, a thin layer of Cr / Ag conductive cathode, a PBD electron transport layer, a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and PBD of 1:1, a C8-BTBT hole transport layer, and an Ag conductive anode, which are stacked in sequence from bottom to top.
[0211] Among them, the structural formula of PBD is Its bandgap is 3.6 eV, and the difference between the highest occupied molecular energy level of C8-BTBT (-5.6 eV) and the lowest unoccupied molecular energy level of PBD (-2.6 eV) is 3 eV;
[0212] The energy level difference between the highest occupied molecular energy level of PBD and the work function of the thin layer Cr / Ag conductive cathode is 2eV.
[0213] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0214] (1) Cleaning the quartz glass substrate and drying it with nitrogen gas;
[0215] (2) a chromium layer with a thickness of 2 nm and a silver layer with a thickness of 5 nm were sequentially evaporated on the cleaned quartz glass substrate to form a thin layer of Cr / Ag conductive cathode;
[0216] (3) treating the quartz glass substrate with the above-mentioned evaporated electrode with UV / ozone for 15 minutes;
[0217] (4) a PBD film with a thickness of 10 nm is evaporated on the Ag layer of the thin-layer Cr / Ag conductive cathode to form a PBD electron transport layer;
[0218] (5) controlling the evaporation rate of C8-BTBT and PBD to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and PBD of 1:1 on the PBD electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 300 nm;
[0219] (6) vapor-depositing a 10 nm thick C8-BTBT film on the bulk heterojunction photosensitive layer to form a C8-BTBT hole transport layer;
[0220] (7) After annealing at 80° C. for 10 minutes in a glove box, a 10 nm thick Ag conductive anode was evaporated on the C8-BTBT hole transport layer through a mask to obtain an organic ultraviolet photodetector.
[0221] The device was tested in air: at -2 V bias, the dark current of the device was 4.5 × 10 -10 A / cm 2 The device's responsivity was measured to be 0.204A / W when the 365nm ultraviolet light was irradiated from the bottom quartz glass substrate, and the responsivity was measured to be 0.142A / W when the 254nm ultraviolet light was irradiated from the bottom quartz glass substrate; the device's response band is 200-375nm, and the UV / visible suppression ratio is greater than 10 4 .
[0222] The UV-visible absorption spectrum of the bulk heterojunction photosensitive layer in this embodiment is as follows: Figure 5The light response spectrum of the organic ultraviolet photodetector provided in this embodiment is shown in Figure 6 shown.
[0223] Embodiment 15
[0224] The present embodiment provides an organic ultraviolet photodetector, comprising a quartz glass substrate, a Cr / Ag conductive cathode, a Bphen electron transport layer, a bulk heterojunction photosensitive layer with a mass ratio of C8-BTBT and Bphen of 1:1, a TAPC hole transport layer, and an Ag conductive anode, which are stacked in sequence from bottom to top.
[0225] Among them, the structural formula of Bphen is Its bandgap is 3.5eV;
[0226] The difference between the highest occupied molecular energy level of C8-BTBT (−5.6 eV) and the lowest unoccupied molecular energy level of Bphen (−2.9 eV) is 2.7 eV;
[0227] The energy level difference between the highest occupied molecular energy level of Bphen and the work function of the Cr / Ag conductive cathode is 2.4 eV;
[0228] The structural formula of TAPC is Its bandgap is 3.5eV.
[0229] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0230] (1) Cleaning the quartz glass substrate and drying it with nitrogen gas;
[0231] (2) a 2 nm thick Cr layer and a 5 nm thick Ag layer were sequentially deposited on the cleaned quartz glass substrate to form a thin layer Cr / Ag conductive cathode;
[0232] (3) treating the quartz glass substrate with the above-mentioned evaporated electrode with UV / ozone for 15 minutes;
[0233] (4) evaporating a 10 nm thick Bphen film on the Ag layer of the thin-layer Cr / Ag conductive cathode to form a Bphen electron transport layer;
[0234] (5) controlling the evaporation rate of C8-BTBT and Bphen to be 1:1, and evaporating a thin film with a mass ratio of C8-BTBT and Bphen of 1:1 on the Bphen electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 300 nm;
[0235] (6) vapor-depositing a TAPC film with a thickness of 10 nm on the surface of the bulk heterojunction photosensitive layer to form a TAPC hole transport layer;
[0236] (7) After annealing at 80° C. for 10 minutes in a glove box, a 10 nm thick Ag conductive anode was evaporated on the TAPC hole transport layer through a mask to obtain an organic ultraviolet photodetector.
[0237] The device was tested in air: at -2 V bias, the dark current of the device was 3.8 × 10 -10 A / cm 2 ; The device's responsivity was measured to be 0.198A / W when irradiated from the bottom quartz glass by 345nm ultraviolet light, and 0.148A / W when irradiated from the bottom quartz glass by 254nm ultraviolet light; The device's response band is 200-360nm, and the UV / visible suppression ratio is greater than 10 4 .
[0238] Example 16
[0239] This embodiment provides an organic ultraviolet photodetector, which is different from Embodiment 15 only in that the bulk heterojunction photosensitive layer is a bulk heterojunction photosensitive layer with a mass ratio of BOPNA and PyDI-BOCF3 of 1:1.
[0240] Among them, the structural formula of BOPNA is: Its bandgap is 4.1eV;
[0241] The structural formula of PyDI-BOCF3 is: Its bandgap is 4.2eV;
[0242] The difference between the highest occupied molecular energy level of BOPNA (-5.6 eV) and the lowest unoccupied molecular energy level of PyDI-BOCF3 (-3.26 eV) is 2.34 eV;
[0243] The energy level difference between the lowest unoccupied molecular energy level of BOPNA and the work function of the Ag conductive anode is 3.5 eV;
[0244] The energy level difference between the highest occupied molecular energy level of PyDI-BOCF3 and the work function of the Cr / Ag conductive cathode is 3.5 eV.
[0245] The method for preparing the organic ultraviolet photodetector comprises the following steps:
[0246] (1) The same as step (1) in Example 15;
[0247] (2) The same as step (2) in Example 15;
[0248] (3) The same as step (3) in Example 15;
[0249] (4) The same as step (4) in Example 15;
[0250] (5) controlling the evaporation rate of BOPNA and PyDI-BOCF3 to be 1:1, and evaporating a thin film of C8-BTBT and Bphen with a mass ratio of 1:1 on the Bphen electron transport layer to form a bulk heterojunction photosensitive layer with a thickness of 300 nm;
[0251] (6) The same as step (6) in Example 15;
[0252] (7) Same as step (7) in Example 15.
[0253] The device was tested in air: at -2 V bias, the dark current of the device was 3.8 × 10 -10 A / cm 2 ; The device's responsivity is 0.198A / W when irradiated with 345nm ultraviolet light from the bottom quartz glass substrate, and 0.148A / W when irradiated with 254nm ultraviolet light from the bottom quartz glass substrate; The device's response band is 200-360nm, and the UV / visible suppression ratio is greater than 10 4 .
[0254] Comparative Example 1
[0255] This embodiment provides a method for preparing an organic ultraviolet photodetector, which is different from Embodiment 5 only in that the bulk heterojunction photosensitive layer is prepared by spin coating and has a thickness of 300 nm.
[0256] The preparation method comprises the steps of:
[0257] (1)-(3) are the same as steps (1)-(3) in Example 5;
[0258] (4) C8-BTBT and PCBM with a mass ratio of 1:1 were dissolved in o-dichlorobenzene to a concentration of 80 mg / ml, a 300 nm bulk heterojunction photosensitive layer was spin-coated on the surface of the PEIE electron transport layer, and annealed at 80 °C in a glove box for 10 min;
[0259] (5)-(6) are the same as steps (5)-(6) in the embodiment.
[0260] The device was tested in air: at -2 V bias, the dark current of the device was 3.6 × 10 -5 A / cm 2 The device responsivity was measured to be 0.0012A / W when the 365nm ultraviolet light was irradiated from the bottom quartz glass substrate, and the device responsivity was measured to be 0.00068A / W when the 254nm ultraviolet light was irradiated from the bottom quartz glass substrate. The UV / visible suppression ratio was greater than 10 2It can be seen that the dark current of the device obtained by preparing the bulk heterojunction photosensitive layer by the spin coating method is higher than that of the device obtained by preparing the bulk heterojunction photosensitive layer by the evaporation method, but the response is low and the UV / visible suppression ratio is low.
[0261] There are no UV photodetectors based on organic semiconductors on the market, and the existing commercial detectors (based on GaN) have a dark current of 10-100pA / cm at a -2V bias. 2 ; The responsivity at 365nm / 254nm is 0.12-0.18A / W and 0.06-0.1A / W respectively; The UV / visible suppression ratio is 10 3 -10 4 It can be seen that the organic ultraviolet photodetector provided by the present invention can be comparable to commercial ultraviolet detectors in terms of light responsivity, detection rate, dark current, detection band and ultraviolet / visible or solar-blind ultraviolet / non-solar-blind ultraviolet suppression ratio, and has the advantages of simple manufacturing process, flexible application integration and low cost.
[0262] In summary, the present invention provides an organic ultraviolet photodetector and a preparation method and related equipment thereof. The p-type organic semiconductor and the n-type organic semiconductor in the bulk heterojunction photosensitive layer both have wide band gaps, and the band gap widths are both greater than or equal to 3.2 eV. Therefore, light detection in the visible blind ultraviolet band (wavelength < 400 nm) or day-blind ultraviolet band (wavelength < 300 nm) can be achieved, and the ultraviolet / visible suppression ratio is greater than 10 4 Since both p-type organic semiconductors and n-type organic semiconductors have wide band gaps, the dark current caused by thermal excitation can be almost ignored. At this time, the main source of the dark current is the injection of electrons and holes from the cathode and anode under reverse bias, respectively. Therefore, in the present invention, the difference between the highest occupied molecular energy level of the p-type organic semiconductor and the lowest unoccupied molecular energy level of the n-type organic semiconductor is maintained at an energy level difference greater than or equal to 1.3 eV, and the potential barrier between the anode or cathode and the bulk heterojunction photosensitive layer is greater than or equal to 2 eV, which effectively blocks the injection of hetero charges in the dark state, ensures high photocurrent, and effectively suppresses the dark current, making the dark current less than 1 nA / cm 2 Based on the above specific p-type organic semiconductor and n-type organic semiconductor materials, the ratio of the two is regulated by precisely controlling the evaporation rate of the two, thereby achieving efficient transport and separation of excitons, as well as efficient transfer of photogenerated carriers, and ultimately achieving extremely low dark current and high sensitivity. In addition, the evaporation process can ensure the stability and repeatability of the film quality, as well as compatibility with current detector manufacturing and chip integration processes.
[0263] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. An organic ultraviolet photodetector, characterized in that: It comprises an anode, a cathode and a bulk heterojunction photosensitive layer arranged between the anode and the cathode, wherein the potential barrier between the anode and the bulk heterojunction photosensitive layer and the potential barrier between the cathode and the bulk heterojunction photosensitive layer are both greater than or equal to 2eV; The bulk heterojunction photosensitive layer comprises at least one p-type organic semiconductor and at least one n-type organic semiconductor, and the band gaps of the p-type organic semiconductor and the n-type organic semiconductor are both greater than or equal to 3.2 eV; The difference between the highest occupied molecular energy level of the p-type organic semiconductor and the lowest unoccupied molecular energy level of the n-type organic semiconductor is greater than or equal to 1.3 eV.
2. The organic ultraviolet photodetector according to claim 1, characterized in that: The highest molecular occupied energy level of the p-type organic semiconductor is -4.9 to -6.0 eV, and the lowest molecular unoccupied energy level of the n-type organic semiconductor is -1.1 to -4.5 eV.
3. The organic ultraviolet photodetector according to claim 1, characterized in that: In the bulk heterojunction photosensitive layer, the mass ratio of the p-type organic semiconductor to the n-type organic semiconductor is 3:1 to 1:
3.
4. The organic ultraviolet photodetector according to claim 1, characterized in that: The organic ultraviolet photodetector further includes a hole transport layer or an electron blocking layer disposed between the anode and the bulk heterojunction photosensitive layer, and the material of the hole transport layer or the electron blocking layer is a p-type semiconductor material.
5. The organic ultraviolet photodetector according to claim 1, characterized in that: The organic ultraviolet photodetector further includes an electron transport layer or a hole blocking layer disposed between the cathode and the bulk heterojunction photosensitive layer, and the material of the electron transport layer or the hole blocking layer is an n-type semiconductor material.
6. The organic ultraviolet photodetector according to claim 1, characterized in that: At least one of the anode and the cathode is a transparent electrode, and the transmittance of the transparent electrode to the ultraviolet band is greater than 80%.
7. The organic ultraviolet photodetector according to claim 1, characterized in that: The p-type organic semiconductor is selected from one of the following structures:
8. The organic ultraviolet photodetector according to claim 1, characterized in that: The n-type organic semiconductor is selected from one of the following structures:
9. A method for preparing the organic ultraviolet photodetector according to any one of claims 1 to 8, characterized in that: Includes steps: providing an anode; forming a bulk heterojunction photosensitive layer on the anode; forming a cathode on the bulk heterojunction photosensitive layer to obtain the organic ultraviolet photodetector; or, providing a cathode; forming a bulk heterojunction photosensitive layer on the cathode; An anode is formed on the bulk heterojunction photosensitive layer to obtain the organic ultraviolet photodetector.
10. The preparation method according to claim 9, characterized in that: forming a bulk heterojunction photosensitive layer on the anode by evaporation; Alternatively, a bulk heterojunction photosensitive layer is formed on the cathode by evaporation.
11. An ultraviolet image sensor, characterized in that: An organic ultraviolet photodetector comprising any one of claims 1 to 8.
12. An electronic device, characterized in that: Includes the ultraviolet image sensor as described in claim 11.