High-performance corrosion-resistant concrete for coastal environment and preparation method of high-performance corrosion-resistant concrete

By using high-performance concrete corrosion-resistant blenders and mineral exciters in a coastal environment, the permeability and chloride permeability of concrete are improved, and the corrosion problem of steel bars caused by seawater erosion in a coastal environment is solved, and the concrete is prolonged. Service life and reduce maintenance costs.

CN119059790AInactive Publication Date: 2024-12-03SHANGHAI CONSTRUCTION GROUP CO LTD

Patent Information

Application Number
CN202411565470.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the coastal environment, concrete is corroded due to seawater erosion and chloride ion penetration, resulting in reduced concrete strength and durability and premature service life attenuation.

Method used

Add high-performance concrete corrosion-resistant blenders and mineral exciters to concrete, including slag powder, fly ash, magnificent powder, liquid sodium silicate, hemihydrate gypsum and sodium sulfate to improve impermeability and chloride resistance Permeability reduces the risk of steel bar corrosion and forms a dense structure through agitation and molding processes.

Benefits of technology

It significantly improves the permeability, chloride ion permeability and durability of concrete, extends the service life of concrete structures, and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to high-performance corrosion-resistant concrete for a coastal environment and a preparation method of the high-performance corrosion-resistant concrete. The concrete comprises the following raw material components in parts by weight: 60-120 parts of cement, 75-140 parts of a concrete corrosion-resistant admixture, 280-350 parts of fine aggregate, 500-600 parts of coarse aggregate, 2-8 parts of a mineral activator, 1-4 parts of a water reducing agent and 50-80 parts of water. According to the concrete, a large-mixing-amount concrete corrosion-resistant admixture is adopted, and the workability and workability of freshly mixed concrete are improved through the micro-aggregate effect of the concrete corrosion-resistant admixture; through the excitation effect of the mineral activator, the pozzolanic activity of the concrete corrosion-resistant admixture is greatly improved, and internal structure gaps of the concrete are filled through the secondary hydration effect of the concrete corrosion-resistant admixture, so that the impermeability and chloride ion permeability resistance of the concrete are improved; and thus, the durability of the concrete, such as sulfate corrosion resistance and freezing resistance, is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to high-performance corrosion-resistant concrete for coastal environments and a preparation method thereof. Background Art

[0002] With the rapid economic development of coastal cities, important projects such as high-rise structures, cross-sea bridges, seaports, submarine tunnels and even offshore oil platforms have emerged rapidly. It is generally believed that the safe service life of concrete buildings (structures) can reach 100 years, but the corrosion environment of concrete in coastal environments is harsh. Due to the influence of various factors such as seawater erosion, steel corrosion, freeze-thaw damage, wave scouring and ice wave impact, it is destroyed prematurely, and the actual service life is far lower than the design requirements. Therefore, the premature decay and failure of the service life of concrete in coastal environments has become a global problem facing today. In order to ensure the long-term stability and safety of concrete structures in coastal environments, a series of technical measures and material optimization are needed. One of the most important effects of the coastal environment on concrete structures is the erosion of seawater and the penetration of chloride ions, which leads to the corrosion of steel bars in concrete, thereby destroying the strength and durability of concrete. Therefore, improving the compactness of the concrete structure itself and its resistance to chloride ion penetration is the key to improving the durability and stability of concrete.

[0003] Therefore, how to provide a high-performance corrosion-resistant concrete for coastal environments and a preparation method thereof is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0004] The present invention provides a high-performance corrosion-resistant concrete for coastal environment and a preparation method thereof. By adding a concrete corrosion-resistant admixture and a mineral activator into the concrete, the concrete impermeability can be effectively improved, the chloride ion permeability can be reduced, the risk of steel bar corrosion can be reduced, and the concrete shrinkage can be reduced, thereby extending the service life of the concrete structure and reducing the maintenance cost.

[0005] In order to solve the above technical problems, the present invention includes the following technical solutions: A high-performance corrosion-resistant concrete for coastal environment, the concrete comprises the following raw material components by weight: 60-120 parts of cement, 75-140 parts of concrete corrosion-resistant admixture, 280-350 parts of fine aggregate, 500-600 parts of coarse aggregate, 2-8 parts of mineral activator, 1-4 parts of water reducer, and 50-80 parts of water; the concrete corrosion-resistant admixture comprises slag powder, fly ash, silica fume and high-grade territorial powder, the fly ash is Class I fly ash, and the SiO 2 The content is greater than or equal to 90%, the specific surface area is greater than or equal to 20000㎡ / kg, and the SiO 2The content is greater than or equal to 50%, and the fineness of 45μm is less than or equal to 5%; the weight ratio is: slag powder 40-60%, fly ash 30-50%, silica fume 0-10%, and kaolin powder 0-10%; the mineral activator includes liquid sodium silicate, hemihydrate gypsum and sodium sulfate.

[0006] Furthermore, the cement is silicate cement of grade PⅡ42.5 or above.

[0007] Furthermore, the fine aggregate is natural river sand with a fineness modulus of 2.4 or above and a mud content of less than or equal to 1.5%.

[0008] Furthermore, the coarse aggregate is continuously graded crushed stone with a particle size of 5 to 25 mm, a needle-like content of less than or equal to 5%, and a mud content of less than or equal to 1%.

[0009] Furthermore, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and its water reducing rate is greater than 25%.

[0010] The present invention also provides a method for preparing high-performance corrosion-resistant concrete for coastal environments, the method comprising the following steps: Step S1, pre-preparing concrete corrosion-resistant admixtures and mineral activators for standby use; Step S2, according to the concrete mix ratio, weigh the required raw materials in proportion, the raw materials including cement, concrete corrosion resistant admixture, coarse aggregate, fine aggregate, mineral activator, water reducing agent and mixing water; Step S3, sequentially adding cement, concrete corrosion resistant admixture, mineral activator and fine aggregate into a mixer and stirring for 30 to 60 seconds, then adding water mixed with admixtures and continuing stirring for 60 to 90 seconds, and then adding coarse aggregate and stirring for 90 to 120 seconds to form a mixture; Step S4, pouring the mixture into a concrete mold, vibrating and compacting it, and forming it; and Step S5: After standard curing, high-performance corrosion-resistant concrete for coastal environment is obtained.

[0011] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present invention provides a high-performance corrosion-resistant concrete for coastal environment and a preparation method thereof. The concrete comprises the following raw material components by weight: 60-120 parts of cement, 75-140 parts of concrete corrosion-resistant admixture, 280-350 parts of fine aggregate, 500-600 parts of coarse aggregate, 2-8 parts of mineral activator, 1-4 parts of water reducer, and 50-80 parts of water. The concrete corrosion-resistant admixture comprises slag powder, fly ash, silica fume and high-grade territorial powder. The fly ash is Class I fly ash, and the SiO 2 The content is greater than or equal to 90%, the specific surface area is greater than or equal to 20000㎡ / kg, and the SiO2 The content is greater than or equal to 50%, and the fineness of 45μm is less than or equal to 5%; the weight ratio is: 40~60% slag powder, 30~50% fly ash, 0~10% silica fume, and 0~10% metakaolin powder. High-performance corrosion-resistant concrete for coastal environment adopts a large amount of concrete corrosion-resistant admixtures, which improves the workability and workability of fresh concrete through its micro-aggregate effect; the volcanic ash activity of the concrete corrosion-resistant admixture is greatly improved by the stimulation of the mineral activator, and the secondary hydration of the concrete corrosion-resistant admixture fills the internal structure gaps of the concrete, making the internal structure of the concrete denser, forming a low-permeability, high-density, low-defect concrete structure, thereby improving the concrete's impermeability and chloride ion permeability, and then improving the concrete's durability such as resistance to sulfate erosion and antifreeze. It has good application value and promotion prospects. DETAILED DESCRIPTION

[0012] The following is a further detailed description of a high performance corrosion resistant concrete for coastal environment and a preparation method thereof provided by the present invention in conjunction with specific embodiments. The advantages and features of the present invention will become more apparent from the following description.

[0013] In the following examples, cement comes from Conch Cement Plant, slag powder comes from Shanghai Baosteel, and fly ash comes from Huaneng Shanghai Shidongkou Power Plant. All materials in the examples and comparative examples are measured by mass.

[0014] The concrete comprises the following raw material components in parts by weight: 60-120 parts of cement, 75-140 parts of concrete corrosion-resistant admixture, 280-350 parts of fine aggregate, 500-600 parts of coarse aggregate, 2-8 parts of mineral activator, 1-4 parts of water reducer and 50-80 parts of water.

[0015] Concrete corrosion-resistant admixtures include slag powder, fly ash, silica fume and high-grade terrestrial powder. The fly ash is Class I fly ash that meets the requirements of the current national standard GB / T 1596-2017. The SiO 2 The content is greater than or equal to 90%, the specific surface area is greater than or equal to 20000㎡ / kg, and the SiO 2 The content is greater than or equal to 50%, and the fineness of 45μm is less than or equal to 5%; the weight ratio is: slag powder 40~60%, fly ash 30~50%, silica fume 0~10%, kaolin powder 0~10%. The corrosion-resistant admixture of concrete composed of slag powder, fly ash, silica fume, kaolin powder, etc. can effectively improve the mechanical properties and durability of concrete.

[0016] Optionally, the mineral activator includes liquid sodium silicate, hemihydrate gypsum and sodium sulfate. The mineral activator composed of liquid sodium silicate, hemihydrate gypsum, sodium sulfate, etc. can improve the volcanic ash activity of the mineral admixture, improve the early strength of the concrete with a large amount of mineral admixture, and improve the compressive strength, impermeability and durability of the concrete.

[0017] Optionally, the cement is silicate cement of grade PⅡ42.5 or above.

[0018] Optionally, the slag powder is granulated blast furnace slag powder of grade S105 that meets the requirements of the current national standard GB / T 18046-2017.

[0019] Optionally, the fine aggregate is natural river sand with a fineness modulus of 2.4 or above and a mud content of less than or equal to 1.5%.

[0020] Optionally, the coarse aggregate is continuously graded crushed stone with a particle size of 5 to 25 mm, a needle-like content of less than or equal to 5%, and a mud content of less than or equal to 1%.

[0021] Optionally, the water reducer is a polycarboxylic acid high-efficiency water reducer, and its water reduction rate is greater than 25%. The polycarboxylic acid high-efficiency water reducer has an electrostatic repulsion effect and a dispersion effect of forming a three-dimensional structure isolation after being adsorbed on particles, and has good compatibility with cementitious materials such as cement, which is beneficial to enhancing the working efficiency of concrete mixtures and reducing water consumption.

[0022] The concrete undergoes hydration reaction with mineral activators, cement and concrete corrosion-resistant admixtures, so that the concrete microstructure is optimized and the pore structure is improved, which is conducive to forming a denser microstructure, improving the concrete's impermeability, mechanical properties and durability, and extending the service life of the concrete structure.

[0023] A method for preparing high-performance corrosion-resistant concrete for coastal environments, the method comprising the following steps: Step S1, pre-preparing concrete corrosion-resistant admixtures and mineral activators for standby use; Step S2, according to the concrete mix ratio, weigh the required raw materials in proportion, the raw materials including cement, concrete corrosion resistant admixture, coarse aggregate, fine aggregate, mineral activator, water reducing agent and mixing water; Step S3, sequentially adding cement, concrete corrosion resistant admixture, mineral activator and fine aggregate into a mixer and stirring for 30 to 60 seconds, then adding water mixed with admixtures and continuing stirring for 60 to 90 seconds, and then adding coarse aggregate and stirring for 90 to 120 seconds to form a mixture; Step S4, pouring the mixture into a concrete mold, vibrating and compacting it, and forming it; and Step S5: After standard curing, high-performance corrosion-resistant concrete for coastal environment is obtained.

[0024] Example 1: A high-performance corrosion-resistant concrete for coastal environment, comprising the following components by mass: 90 parts of cement, 110 parts of concrete corrosion-resistant admixture, 330 parts of fine aggregate, 560 parts of coarse aggregate, 7 parts of mineral activator, 2.5 parts of water reducer, and 72 parts of mixing water. Among them, 110 parts of concrete corrosion-resistant admixture contain 55 parts of slag powder, 50 parts of fly ash, and 5 parts of high-altitude soil; 7 parts of mineral activator contain 3.5 parts of liquid sodium silicate, 2.5 parts of hemihydrate gypsum, 0.5 parts of sodium sulfate, and 0.5 parts of others.

[0025] The high-performance corrosion-resistant concrete for coastal environment was prepared according to the aforementioned preparation method of high-performance corrosion-resistant concrete for coastal environment, with a total mixing time of 250s, thereby preparing high-performance corrosion-resistant concrete for coastal environment.

[0026] Example 2: A high-performance corrosion-resistant concrete for coastal environment, comprising the following components by mass: 100 parts of cement, 100 parts of concrete corrosion-resistant admixture, 333 parts of fine aggregate, 561 parts of coarse aggregate, 6.5 parts of mineral activator, 2.3 parts of water reducer, and 72 parts of mixing water. Among them, 100 parts of concrete corrosion-resistant admixture contain 50 parts of slag powder, 45.5 parts of fly ash, and 4.5 parts of high-altitude land; 6.5 parts of mineral activator contain 3.2 parts of liquid sodium silicate, 2.3 parts of hemihydrate gypsum, 0.5 parts of sodium sulfate, and 0.5 parts of others.

[0027] The high-performance corrosion-resistant concrete for coastal environment was prepared according to the aforementioned preparation method of high-performance corrosion-resistant concrete for coastal environment, with a total mixing time of 250s, thereby preparing high-performance corrosion-resistant concrete for coastal environment.

[0028] Example 3: A high-performance corrosion-resistant concrete for coastal environment, comprising the following components by mass: 110 parts of cement, 90 parts of concrete corrosion-resistant admixture, 336 parts of fine aggregate, 561 parts of coarse aggregate, 6 parts of mineral activator, 2.0 parts of water reducer, and 72 parts of mixing water. Among them, 90 parts of concrete corrosion-resistant admixture contain 45 parts of slag powder, 40.9 parts of fly ash, and 4.1 parts of high-altitude land; 6 parts of mineral activator contain 3.0 parts of liquid sodium silicate, 2.2 parts of hemihydrate gypsum, 0.4 parts of sodium sulfate, and 0.4 parts of others.

[0029] The high-performance corrosion-resistant concrete for coastal environment was prepared according to the aforementioned preparation method of high-performance corrosion-resistant concrete for coastal environment, with a total mixing time of 250s, thereby preparing high-performance corrosion-resistant concrete for coastal environment.

[0030] Example 4: A high-performance corrosion-resistant concrete for coastal environment, comprising the following components by mass: 90 parts of cement, 110 parts of concrete corrosion-resistant admixture, 330 parts of fine aggregate, 560 parts of coarse aggregate, 7 parts of mineral activator, 2.5 parts of water reducer, and 72 parts of mixing water. Among them, 110 parts of concrete corrosion-resistant admixture contain 55 parts of slag powder and 55 parts of fly ash; 7 parts of mineral activator contain 3.5 parts of liquid sodium silicate, 2.5 parts of hemihydrate gypsum, 0.5 parts of sodium sulfate, and 0.5 parts of others.

[0031] The high-performance corrosion-resistant concrete for coastal environment was prepared according to the aforementioned preparation method of high-performance corrosion-resistant concrete for coastal environment, with a total mixing time of 250s, thereby preparing high-performance corrosion-resistant concrete for coastal environment.

[0032] Example 5: A high-performance corrosion-resistant concrete for coastal environment, comprising the following components by mass: 90 parts of cement, 110 parts of concrete corrosion-resistant admixture, 329 parts of fine aggregate, 560 parts of coarse aggregate, 7 parts of mineral activator, 3 parts of water reducer, and 72 parts of mixing water. Among them, 110 parts of concrete corrosion-resistant admixture contain 55 parts of slag powder, 50 parts of fly ash, and 5 parts of silica powder; 7 parts of mineral activator contain 3.5 parts of liquid sodium silicate, 2.5 parts of hemihydrate gypsum, 0.5 parts of sodium sulfate, and 0.5 parts of others.

[0033] The high-performance corrosion-resistant concrete for coastal environment was prepared according to the aforementioned preparation method of high-performance corrosion-resistant concrete for coastal environment, with a total mixing time of 250s, thereby preparing high-performance corrosion-resistant concrete for coastal environment.

[0034] Comparative example: ordinary concrete, compared with Examples 1 to 4, the difference is that the comparative example admixture uses Grade II fly ash and no mineral activator is used; it includes the following components in parts by mass: 170 parts of cement, 30 parts of fly ash, 353 parts of fine aggregate, 571 parts of coarse aggregate, 2 parts of water reducer, and 72 parts of mixing water.

[0035] The high-performance corrosion-resistant concrete for coastal environment was prepared according to the aforementioned preparation method, with a total mixing time of 250 seconds, thereby preparing ordinary concrete.

[0036] The test results of the concrete in Examples 1 to 5 and the comparative example are shown in Tables 1 and 2.

[0037] Table 1 Workability of high performance corrosion resistant concrete for coastal environment.

[0038]

[0039] It can be seen from Table 1 that, compared with the comparative example, the slump of the high performance corrosion resistant concrete for coastal environment of Examples 1 to 5 is basically the same, but the cohesiveness and water retention are good.

[0040] Table 2 Mechanical properties and durability of high performance corrosion resistant concrete for coastal environment.

[0041]

[0042] As shown in Table 2, compared with the comparative example, the compressive strength of the high-performance corrosion-resistant concrete for coastal environment in Examples 1 to 5 is basically the same, and the electric flux, Cl - The anti-seepage performance represented by the permeability coefficient and the water seepage height has been significantly improved, the anti-sulfate erosion performance is significantly better than the control group, and the anti-freeze performance is slightly better than the control group.

[0043] In summary, high-performance corrosion-resistant concrete for coastal environment uses a large amount of concrete corrosion-resistant admixtures, which improves the workability and workability of fresh concrete through its micro-aggregate effect; the volcanic ash activity of the concrete corrosion-resistant admixture is greatly improved by the stimulation of the mineral activator, and the internal structure voids of the concrete are filled through the secondary hydration of the concrete corrosion-resistant admixture, making the internal structure of the concrete denser, forming a low-permeability, high-density, low-defect concrete structure, thereby improving the concrete's impermeability and chloride ion permeability, and then improving the concrete's durability such as resistance to sulfate erosion and frost resistance. It has good application value and promotion prospects.

[0044] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. The above embodiments only express several embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high performance corrosion resistant concrete for coastal environment, It is characterized in that The concrete comprises the following raw material components by weight: 60-120 parts of cement, 75-140 parts of concrete corrosion-resistant admixture, 280-350 parts of fine aggregate, 500-600 parts of coarse aggregate, 2-8 parts of mineral activator, 1-4 parts of water reducer, 50-80 parts of water, the concrete corrosion-resistant admixture comprises slag powder, fly ash, silica fume and high-grade territorial powder, the fly ash is Class I fly ash, and the SiO 2 The content is greater than or equal to 90%, the specific surface area is greater than or equal to 20000㎡ / kg, and the SiO 2 The content is greater than or equal to 50%, and the fineness of 45μm is less than or equal to 5%; the weight ratio is: slag powder 40-60%, fly ash 30-50%, silica fume 0-10%, and kaolin powder 0-10%; the mineral activator includes liquid sodium silicate, hemihydrate gypsum and sodium sulfate.

2. The high performance corrosion resistant concrete for coastal environment according to claim 1, It is characterized in that The cement is silicate cement of grade PⅡ42.5 or above.

3. The high performance corrosion resistant concrete for coastal environment according to claim 1, It is characterized in that The fine aggregate is natural river sand with a fineness modulus of 2.4 or above and a mud content of less than or equal to 1.5%.

4. The high performance corrosion resistant concrete for coastal environment according to claim 1, It is characterized in that The coarse aggregate is continuously graded crushed stone with a particle size of 5 to 25 mm, a needle-like content of less than or equal to 5%, and a mud content of less than or equal to 1%.

5. The high performance corrosion resistant concrete for coastal environment according to claim 1, It is characterized in that The water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and its water reducing rate is greater than 25%.

6. A method for preparing high-performance corrosion-resistant concrete for coastal environment according to any one of claims 1 to 5, It is characterized in that The method comprises the following steps: Step S1, pre-preparing concrete corrosion-resistant admixtures and mineral activators for standby use; Step S2, according to the concrete mix ratio, weigh the required raw materials in proportion, the raw materials including cement, concrete corrosion resistant admixture, coarse aggregate, fine aggregate, mineral activator, water reducing agent and mixing water; Step S3, sequentially adding cement, concrete corrosion resistant admixture, mineral activator and fine aggregate into a mixer and stirring for 30 to 60 seconds, then adding water mixed with admixtures and continuing stirring for 60 to 90 seconds, and then adding coarse aggregate and stirring for 90 to 120 seconds to form a mixture; Step S4, pouring the mixture into a concrete mold, vibrating and compacting it, and forming it; as well as Step S5: After standard curing, high-performance corrosion-resistant concrete for coastal environment is obtained.

Citation Information

Patent Citations

  • High-strength corrosion-resistant prestress concrete pipe pile

    CN108147723A

  • Maritime work admixture

    CN110698102A

  • High-performance marine concrete with excellent durability and preparation method thereof

    CN112209687A

  • Concrete suitable for chlorine salt dry and wet environment and preparation method

    CN116986866A

  • Corrosion proof high performance marine concrete and its production

    CN1712383A

Cited By

  • A salt spray solid particle concentration monitoring system for coastal environments

    CN120253597B

  • Salt mist solid particle concentration monitoring method for simulating coastal environment

    CN120594348A

  • Salt mist solid particle concentration monitoring system for simulating coastal environment

    CN120594349A

  • Salt mist solid particle concentration monitoring method for analyzing coastal environment

    CN120594350A

  • Salt mist solid particle concentration monitoring system for analyzing coastal environment

    CN120594351A