Cutting-resistant and anti-fatigue composition for tires of passenger cars and preparation method of cutting-resistant and anti-fatigue composition
By adding pyrazolinone and tetrazine compounds to the rubber composition and using specific process treatment, the problem of contradiction between rolling resistance and cutting resistance and tear resistance in the prior art is solved, and the tires in passenger cars are realized The effect of reducing rolling resistance and improving cutting resistance and tear resistance.
Patent Information
- Application Number
- CN202411562390.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing rubber compositions are difficult to improve the cutting and tear resistance of passenger vehicle tires while reducing rolling resistance, and improving one performance is often accompanied by losses of other properties, resulting in cutting and tear resistance in low rolling resistance tires. Weak cracking performance.
Using a composition including diene rubber, pyrazolinone compound, tetraazine compound, reinforcement filler, silane coupling agent, vulcanization accelerator, antioxidant, etc., it is treated through specific mixing and vulcanization reactions. A rubber composition with excellent cutting resistance and damage resistance is formed.
It realizes the cutting and tear resistance of the rubber composition while reducing rolling resistance, extends the service life of the tire, reduces heat generation, and improves the overall fatigue resistance.
Smart Images

Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the field of rubber technology, and more particularly to a composition for passenger car tires that is resistant to cutting and fatigue and a preparation method thereof. Background Art
[0002] During the driving process, due to the friction, shearing, cutting and bumping between the tire and the ground, the tire tread will have problems such as chipping, cracking, etc., which will reduce the service life of the tire. Especially for new energy vehicles, compared with fuel vehicles, the weight is increased, the torque and acceleration and deceleration are increased during starting and braking, and the rolling resistance and heat generation of the tires are relatively low. Therefore, the tires are more likely to have problems such as tread cracks, groove bottom cracks, chipping and chipping. Improving the tire's anti-destructive properties such as cutting resistance and tearing resistance will help improve this problem. At the same time, reducing the rolling resistance or heat generation of the tire can further improve the durability of the tire.
[0003] There are often limitations in performance when changing the type of rubber or adjusting the amount of white carbon black and carbon black used in traditional ways. Since low rolling resistance requires the rubber material to have lower energy dissipation (hysteresis loss), and high cut and tear resistance under large deformation requires higher energy dissipation capacity, low rolling resistance and high cut and tear resistance are contradictory. While reducing rolling resistance, cut and tear resistance often deteriorates, and often when improving one performance, it is accompanied by the loss of other performances, which makes it difficult to improve the cut and tear resistance of low rolling resistance tires. Therefore, it is currently difficult to achieve both low rolling resistance and high cut and tear resistance at the same time.
[0004] Patent publication number CN112533991B discloses rubber compositions, rubber materials and their uses, rubber compositions that can exhibit low heat generation, tear strength and durability; and rubber compositions with excellent low heat generation, tear strength and durability. In the embodiments where the amount of natural rubber (NR) or polyisoprene rubber (IR) is 100 parts or more than 50 parts, pyrazolone compounds have good low heat generation, tear strength and durability; however, there is no embodiment data showing that when the amount of synthetic rubber such as styrene-butadiene copolymer rubber (SBR styrene-butadiene rubber) exceeds 50 parts and the amount of white carbon black is higher than 50 parts, low rolling resistance and improved tear strength.
[0005] Patent publications CN110392713B, CN108026332B, CN110382611B, CN110382612B, CN110382554B, and CN110461931B disclose rubber compositions and tires. By combining a specific rubber component, a tetrazine compound represented by the general formula (1) or its salt, and carbon black, a rubber composition that can not only impart excellent low heat generation to the tire, but also impart excellent wear resistance to the tire can be provided. However, these patent publications do not provide any description or example data description of the cut and tear resistance. In addition, the tire made by using the rubber composition of the invention can not only reduce the rolling resistance of the tire, reduce the heat generation of the tire, but also improve the wear resistance, thereby providing a low fuel consumption tire for large vehicles. However, wear resistance belongs to the anti-wear performance under small deformation under mild road conditions, which is not inconsistent with the low heat generation under high dispersion of fillers in rubber, but is inconsistent with the rubber action mechanism of cut and tear resistance under large deformation under harsh road conditions. Therefore, the anti-destructive properties such as cut resistance and tear resistance of tires made of this rubber composition are weak or even deteriorate.
[0006] Therefore, how to provide a rubber composition and a preparation method thereof that can improve the cut resistance and damage resistance while reducing the rolling resistance is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0007] In order to overcome the above defects of the prior art, the present invention provides a composition for passenger car tires with cut resistance and fatigue resistance and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0008] To achieve the above object, the present invention provides the following technical scheme: a composition for cut resistance and fatigue resistance of passenger car tires and a preparation method thereof, comprising the following raw materials in parts by weight: 100 parts of diene rubber, 0.2-1.5 parts of pyrazolone compounds, 0-1.5 parts of tetrazine compounds, 20-150 parts of reinforcing fillers, 2-20 parts of silane coupling agents, vulcanization accelerators, vulcanizing agents, antioxidants, vulcanization activators, resins and plasticizers; The structure of the tetrazine compound is: (1) Wherein X1 and X2 represent a heterocyclic group which may have a substituent, and the substituent is an alkyl group, an aralkyl group, an aryl group or a heterocyclic group; The structure of the pyrazolone compound is: (2) (3) Among them, R1, R2, R3, and R4 are the same or different, representing a hydrogen atom, an alkyl group, an aralkyl group, an aryl group or a heterocyclic group; R3 and R4 can be connected to form an alkylene group, and any two of R2, R3 and R4 can be connected together to form an alkylene group; R5, R7, R8 are the same or different, representing a hydrogen atom, an alkyl group, an aralkyl group, an aryl group or a heterocyclic group; R6 represents an alkyl group, an aralkyl group, an aryl group or a heterocyclic group, and each of these groups can have one or more substituents, and the substituents are alkyl groups, aralkyl groups, aryl groups or heterocyclic groups.
[0009] Preferably, the diene rubber is any one or more combinations of modified or unmodified natural rubber, polyisoprene rubber, polybutadiene rubber, butadiene rubber, styrene-butadiene copolymer rubber, ethylene-propylene-diene monomer copolymer, styrene-isoprene-styrene terblock copolymer rubber, and styrene-butadiene-styrene terblock copolymer rubber.
[0010] Preferably, the styrene-butadiene copolymer rubber contains 5%-40%wt of styrene, and the styrene-butadiene copolymer rubber is a combination of one or more of the following elastomeric substances: unmodified solution-polymerized styrene-butadiene rubber, unmodified emulsion-polymerized styrene-butadiene rubber, end-group-modified solution-polymerized styrene-butadiene rubber, end-group-modified emulsion-polymerized styrene-butadiene rubber, main chain-modified solution-polymerized styrene-butadiene rubber and main chain-modified emulsion-polymerized styrene-butadiene rubber.
[0011] Preferably, the diene rubber is a combination of any one or more of modified or unmodified styrene-butadiene copolymer rubber and polybutadiene rubber, and the amount of the styrene-butadiene copolymer rubber and polybutadiene rubber is 50-100 parts, preferably 60-100 parts.
[0012] Preferably, the diene rubber is a combination of any one or more of modified or unmodified natural rubber and polyisoprene rubber, and the amount of the natural rubber and polyisoprene rubber is 0-50 parts, preferably 0-40 parts.
[0013] The beneficial effects of adopting the above technical solution are as follows: the above rubber is used to improve the cut resistance and damage resistance and reduce the rolling resistance of the tire; among the styrene-butadiene rubbers, solution-polymerized styrene-butadiene rubber is more preferred, because the solution-polymerized styrene-butadiene rubber has lower rolling resistance, and after adding pyrazolone and / or tetrazine compounds or being modified, the balance between cut resistance, rolling resistance and processing performance is better; among the polybutadiene rubbers, the nickel catalyst system, lithium catalyst system and rare earth catalyst system are preferred, and the addition of modified polybutadiene rubber can effectively balance the wear resistance, rolling resistance, processing performance and aging resistance and fatigue crack propagation performance.
[0014] Preferably, the pyrazolone compound is a combination of any one or more of 3-methyl-5-pyrazolone, 3-phenyl-5-pyrazolone, 3-ethyl-5-pyrazolone, 3-propyl-5-pyrazolone, and 3-butyl-5-pyrazolone, and the amount of the pyrazolone compound is 0.3-1.2 parts, preferably 0.3-0.8 parts.
[0015] Preferably, the tetrazine compound is any one or more of 3,6-bis(2-pyridyl)-1,2,4,5-tetrazine, 3,6-bis(3-pyridyl)-1,2,4,5-tetrazine, and 3,6-bis(4-pyridyl)-1,2,4,5-tetrazine, and the amount of the tetrazine compound is 0-1.2 parts, preferably 0.3-0.8 parts.
[0016] The beneficial effects of the above technical solution are as follows: the above pyrazolone compounds are used to graft-modify styrene-butadiene rubber and natural rubber, and are complexed with metal oxides to form a weak sacrificial network in the diene rubber system, which can preferentially resist external force damage and improve the anti-cutting, anti-tearing and other anti-destruction capabilities of the rubber composition; the tetrazine compounds are used to graft-modify styrene-butadiene rubber, while improving the dispersion of fillers and reducing rolling resistance. The combination of pyrazolone compounds and tetrazine compounds improves the anti-destruction performance of the final product and further reduces the rolling resistance of the rubber composition; the pyrazolone compounds and tetrazine compounds have a certain synergistic effect, further improving the anti-destruction performance such as cut resistance.
[0017] Preferably, the reinforcing filler is any one or more combinations of modified or unmodified carbon black, acetylene black, white carbon black, carbon nanotubes, graphite, and graphene, and the amount of white carbon black in the reinforcing filler is 50-150 parts, and the amount of carbon black is 0-50 parts.
[0018] Preferably, the specific surface area of the carbon black is 20-160m 2 / g, the specific surface area of white carbon is 60-250m 2 More preferably, the specific surface area of the carbon black is 40-140m 2 / g, the specific surface area of white carbon black is 90-200m 2 / g.
[0019] More preferably, the carbon black is one or a combination of N110, N121, N134, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990 and N991; the iodine absorption value of the above carbon black is 5-150g / kg, and the DBP absorption value is 30-150cm3 / 100g.
[0020] Preferably, the carbon black is 0-30 parts and the white carbon black is 50-120 parts.
[0021] The silane coupling agent is any one or more of bis-[3-(triethoxysilyl)propyl]-tetrasulfide (Si 69), bis-[3-(triethoxysilyl)propyl]-disulfide (Si75), 3-octanoylthio-1-propyltriethoxysilane (NXT), γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane) (Si747) and mercaptoalkoxy-ethoxysilane (Si363), preferably bis-[3-(triethoxysilyl)propyl]-tetrasulfide (Si69), bis-[3-(triethoxysilyl)propyl]-disulfide (Si75), 3-octanoylthio-1-propyltriethoxysilane (NXT), and more preferably bis-[3-(triethoxysilyl)propyl]-tetrasulfide (Si 69), bis-[3-(triethoxysilyl)propyl]-disulfide (Si75), 3-octanoylthio-1-propyltriethoxysilane (NXT), the amount of the silane coupling agent is 3-17 parts, preferably 4-15 parts.
[0022] The beneficial effect of adopting the above technical solution: in the present invention, by adjusting the types and amounts of white carbon black, carbon black and silane coupling agent, the low rolling resistance and improved anti-damage performance of the final product can be better balanced.
[0023] The vulcanization accelerator is a combination of any one or more of thiazoles, thiurams, sulfenamides, dithiocarbamates, xanthates, guanidines and thioureas; preferably diphenylguanidine and N-cyclohexane-2-benzothiazole sulfenamide; the amount of the vulcanization accelerator is 0.5-4 parts, preferably 0.8-3 parts, and more preferably 1-2.5 parts.
[0024] The vulcanizing agent is sulfur, and the amount of the vulcanizing agent is 0.5-5 parts, preferably 0.8-4 parts, and more preferably 1-3 parts.
[0025] The rubber composition for improving the cut resistance and damage resistance of passenger car tires and reducing rolling resistance and the preparation method thereof also include an antioxidant, a vulcanization activator zinc oxide and stearic acid, a resin and a plasticizer.
[0026] A composition for cutting resistance and fatigue resistance of passenger car tires and a preparation method thereof, comprising the following steps: step (1) weighing various raw materials: the raw materials include diene rubber, pyrazolone compound, tetrazine compound reinforcing filler, silane coupling agent, vulcanization accelerator, vulcanizing agent, antioxidant, vulcanization activator, resin and plasticizer; Step (2) mixing diene rubber, pyrazolone compound, tetrazine compound, antioxidant, reinforcing filler, silane coupling agent, and vulcanization accelerator diphenylguanidine, and performing a mixing reaction at 120-180° C. for 60-300 seconds, and cooling the mixture to obtain material A; Step (3) mixing the remaining raw materials except the vulcanizing agent and the vulcanization accelerator with material A, and performing a mixing reaction at 120-180° C. for 60-300 seconds, and then cooling to obtain material B; Step (4) adds a vulcanizing agent and a vulcanization accelerator to material B, mixes and discharges the material, and then performs a vulcanization reaction to obtain a rubber composition that can improve anti-damage performance and reduce heat generation.
[0027] Preferably, in step (2) and step (3), the mixing reaction time is 2-10 min, the discharge temperature is 120-180° C., the vulcanization temperature is 130-180° C., the vulcanization time is 10-200 min, and the vulcanization process is carried out in a mold heated by oil bath or electric heating.
[0028] Preferably, in the above preparation method, part or all of the carbon black in the reinforcing filler can be added in step (2) or step (3); part or all of the white carbon black in the reinforcing filler can be added in step (2) or step (3); and part or all of the silane coupling agent can be added in step (2) or step (3) according to the proportion of white carbon black added; In the above preparation method, the vulcanization accelerator diphenylguanidine can be added partially or completely in step (2) or step (3) according to the ratio of white carbon black added; The tetrazine compound is entirely added in step (2), and the pyrazolone compound and the antioxidant may be partially or entirely added in step (2), step (3), or step (4).
[0029] A passenger car tire is prepared by using the above-mentioned composition for cutting resistance and fatigue resistance of passenger car tires and the preparation method thereof.
[0030] The present invention provides a composition for passenger car tires that is resistant to cutting and fatigue and a preparation method thereof, which has the following beneficial effects: In the present invention, by adding a small amount of tetrazine compounds and pyrazolone compounds and applying the optimized rubber refining process that conforms to the reaction of tetrazine compounds, pyrazolone compounds and rubber, the composition can simultaneously reduce the hysteresis loss and heat generation of the rubber and improve the anti-destructive properties such as cutting resistance and tearing resistance; the preparation method of the present invention is simple to operate and has strong practicality. DETAILED DESCRIPTION
[0031] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work shall fall within the scope of protection of the present invention.
[0032] The standards and methods for testing the rubber composition of the present invention in the following examples are as follows: 1) Mooney viscosity: Refer to ASTM D1646-2007, test conditions are ML (1+4) 100°C. The larger the index, the higher the Mooney viscosity.
[0033] 2) Mooney scorch: Refer to ASTM D1646-2007, the test temperature is 130 degrees Celsius. The larger the index, the longer the scorch time.
[0034] 3) Hardness: Shore hardness test, refer to ASTM D2240-2010. The larger the index, the higher the hardness.
[0035] 4) MA100: 100% tensile modulus test, refer to ASTM D412-2006, take the modulus when the elongation is 100%. The test environment temperature is 23±2℃. The larger the index, the higher the tensile modulus.
[0036] 5) MA300: 300% tensile modulus test, refer to ASTM D412-2006, take the modulus when the elongation is 300%. The test environment temperature is 23±2℃. The larger the index, the higher the tensile modulus.
[0037] 6) Tensile strength and elongation at break: refer to ASTM D412-2006, the sample is dumbbell-shaped, the test speed is 500mm / min, and the test environment temperature is 23±2℃. The larger the index, the higher the tensile strength.
[0038] 7) Hysteresis loss factor: Tested using Metravib DMA, temperature 25°C, frequency 10Hz, dynamic deformation 0.07%-50%, plane shear mode. Using the tand(max) standard, the smaller the index, the smaller the hysteresis loss and the lower the heat generation.
[0039] 8) Tear strength: refer to ASTM D624-00 (2012), the sample is torn at right angles, the test speed is 500mm / min, and the test environment temperature is 23±2℃. The larger the index, the higher the tear strength and the better the tear resistance.
[0040] 9) Cutting loss: The test was conducted using an RCC-I rubber dynamic cutting tester, with a rotation speed of 720 rpm, a cutting frequency of 120 times / min, and a cutting time of 20 minutes. The smaller the index, the smaller the cutting loss and the better the cutting resistance.
[0041] The raw materials used in the embodiments of the present invention are as follows: Natural rubber: STR20, Sinochem International (Holdings) Co., Ltd. NS624 (styrene-butadiene rubber): Zeon Corporation SSBR2564S (styrene-butadiene rubber): Dushanzi Petrochemical Company SOL5251H (styrene-butadiene rubber): Kumho Chemical BR9000 (polybutadiene rubber) Sinopec Qilu Petrochemical Company Tetrazines: 3,6-Bis(2-pyridyl)-1,2,4,5-tetrazine, Otsuka Chemical Co., Ltd. Pyrazolone compounds: 3-Methyl-5-pyrazolone, TCI (Shanghai) Chemical Industry Development Co., Ltd. HD165MP (white carbon black): Wuxi Quecheng Silicon Co., Ltd. N234, N330 (Carbon Black): Cabot Carbon Black Vivatec700: Hansheng Chemical Si69: Evonik Specialty Chemicals (Shanghai) Co., Ltd. 6PPD (antioxidant): Shandong Shangshun Chemical Co., Ltd. TMQ (antioxidant): Shandong Shangshun Chemical Co., Ltd. SA (stearic acid): Sichuan Tianyu Oil Chemical Co., Ltd. Antilux111 (microcrystalline wax antioxidant): LANXESS DPG: Shandong Shangshun Chemical Co., Ltd. ZnO (zinc oxide): Dalian Zinc Oxide Co., Ltd. CBS (N-cyclohexyl-2-benzothiazole sulfenamide): Shandong Shangshun Chemical Co., Ltd. S (sulfur): Shandong Shangshun Chemical Co., Ltd.
[0042] Example 1 The raw materials used in Comparative Example 1-1 and Examples 1-1 to 1-6 of the present invention are shown in the following table, all in parts by mass: Wherein, Examples 1-1, 1-2 and 1-3 respectively added different amounts of pyrazolone compounds, 1-4 and 1-5 respectively added different amounts of tetrazine compounds, Example 1-7 used a pyrazolone compound and a tetrazine compound in combination, and Comparative Example 1-1 did not add pyrazolone compounds and tetrazine compounds.
[0043] Table 1: Formulations of rubber compositions of Comparative Example 1-1 and Examples 1-1 to 1-6 Material Comparative Example 1-1 Example 1-1 Example 1-2 Examples 1-3 Examples 1-4 Examples 1-5 Examples 1-6 NS624 60 60 60 60 60 60 60 STR20 15 15 15 15 15 15 15 BR9000 25 25 25 25 25 25 25 HD165MP 50 50 50 50 50 50 50 Si69 4 4 4 4 4 4 4 N330 4 4 4 4 4 4 4 DPG 0.6 0.6 0.6 0.6 0.6 0.6 0.6 6PPD 2 2 2 2 2 2 2 Antilux111 1.5 1.5 1.5 1.5 1.5 1.5 1.5 ZnO 2 2 2 2 2 2 2 SA 2 2 2 2 2 2 2 3,6-Bis(2-pyridyl)-1,2,4,5-tetrazine 0.5 0.8 0.5 3-Methyl-5-pyrazolone 0.3 0.6 1 0.6 CBS 2 2 2 2 2 2 2 S 1 1 1 1 1 1 1 The above schemes all adopt the following preparation method: Step (1) weighing the raw materials according to the weight in Table 1; Step (2) mixing the rubber for 30 seconds, adding 3-methyl-5-pyrazolone, 3,6-bis(2-pyridyl)-1,2,4,5-tetrazine, 20 parts of white carbon black HD165MP, 2 parts of silane coupling agent Si69, 0.6 parts of vulcanization accelerator DPG, and 1 part of antioxidant 6PPD, mixing and reacting at 130-150° C. for 120 seconds, and debonding at 150° C. to obtain material A; Step ( 3) mixing the remaining raw materials except the vulcanizing agent and the vulcanization accelerator with the material A, performing a mixing reaction at 140-150° C. for 120 seconds, and performing a rubber discharge at 150° C. to obtain the material B; step (4) adding the vulcanizing agent and the vulcanization accelerator to the material B, mixing for about 180 seconds in an internal mixer, discharging the material at 110° C., and then performing a vulcanization reaction at 170° C. for 15 minutes, to obtain a rubber composition for passenger car tires with improved cut resistance and damage resistance and reduced rolling resistance.
[0044] The rubber compositions of the comparative examples and the examples were tested for cut resistance, tear strength, tensile strength, etc. The test results are shown in Table 2.
[0045] Table 2: Test results of rubber compositions of Comparative Example 1-1 and Examples 1-1 to 1-6 Test Item* Comparative Example 1-1 Example 1-1 Example 1-2 Examples 1-3 Examples 1-4 Examples 1-5 Examples 1-6 Mooney viscosity 100 106 115 117 126 128 125 Scorch time 100 104 124 123 118 113 105 hardness 100 98 95 93 97 95 97 MA100 100 86 81 78 106 108 95 MA300 100 85 70 67 104 106 89 Tensile Strength 100 100 92 95 95 95 101 Elongation at break 100 108 116 119 93 90 109 Tear strength 100 108 124 132 91 91 130 Hysteresis loss factor 100 100 100 109 74 71 80 Cutting loss 100 79 64 61 95 98 80 *The test results of rubber compositions are expressed in the form of indices. The calculation formula is: test item = (embodiment / comparative example 1-1) × 100.
[0046] It can be seen from Table 2 that compared with Comparative Example 1-1, the tear strength of Examples 1-1, 1-2, and 1-3 are increased by 8%, 24%, and 32%, respectively, the cutting loss is reduced by 21%, 36%, and 39%, respectively, and the elongation at break is increased by 8%, 15%, and 19%, respectively, indicating that with the addition of the pyrazolone compound, the tear strength, cutting loss, and elongation at break of the rubber composition are significantly improved, and the fatigue resistance and cut resistance are improved; compared with Comparative Example 1-1, the hysteresis loss factor of Example 1-3 is 9% higher, and the hysteresis loss factors of Examples 1-1 and 1-2 have no obvious change, indicating that with the addition of the pyrazolone compound, the hysteresis loss of the rubber composition may increase, and the rolling resistance and heat generation will increase.
[0047] Compared with Comparative Example 1-1, the hysteresis loss factors of Examples 1-4 and 1-5 decreased by 26% and 29%, respectively, that is, the addition of tetrazine compounds can significantly reduce the hysteresis loss of the rubber composition and reduce heat generation. Compared with Comparative Example 1-1, the cutting loss of Examples 1-4 and 1-5 decreased by less than 5%, and there was no improvement effect on the cut resistance. Compared with Comparative Example 1-1, the elongation at break and tear strength of Examples 1-4 and 1-5 decreased.
[0048] Compared with Comparative Example 1-1, the elongation at break and tear strength of Example 1-6 increased by 9% and 30% respectively, the cutting loss decreased by 20%, and the hysteresis loss factor decreased by 20%. Compared with Example 1-2, the hysteresis loss factor of Example 1-6 decreased by 20%. This indicates that when the pyrazolone compound and the tetrazine compound are added simultaneously, the cutting and tearing resistance of the rubber composition is improved, and the hysteresis loss is further reduced.
[0049] The data in Table 2 show that when the pyrazolone compound is added alone, the elongation at break and tear strength of the rubber composition can be significantly improved, the cutting loss can be reduced, and the fatigue resistance, tear resistance and cutting resistance can be significantly improved, but the hysteresis loss and heat generation may increase. When the tetrazine compound is added to the pyrazolone compound, the fatigue resistance, tear resistance and cutting resistance of the rubber composition are significantly improved, while the hysteresis loss, rolling resistance and heat generation are further reduced. Example
[0050] The raw materials used in Comparative Examples 2-1 to 2-3 and Examples 2-1 to 2-7 of the present invention are shown in the following table, all in parts by mass: Comparative Examples 2-1, 2-2, and 2-3 have different amounts of white carbon black filled, and no pyrazolone compound and tetrazine compound are added. Examples 2-1 and 2-2 are based on Comparative Example 2-1, and pyrazolone compound is added alone, and tetrazine compound is used in combination. Examples 2-3, 2-4, and 2-5 are based on Comparative Example 2-2, and pyrazolone compound and tetrazine compound are added and used in combination. Examples 2-6 and 2-7 are based on Comparative Example 2-3, and pyrazolone compound and tetrazine compound are added and used in combination.
[0051] Table 3: Formulations of rubber compositions of Comparative Example 2-1 and Examples 2-1 to 2-7 Material Comparative Example 2-1 Comparative Example 2-2 Comparative Examples 2-3 Example 2-1 Example 2-2 Example 2-3 Embodiment 2-4 Embodiment 2-5 Embodiment 2-6 Embodiment 2-7 SOL5251H 75 75 75 75 75 75 75 75 75 75 BR9000 15 15 15 15 15 15 15 15 15 15 STR20 10 10 10 10 10 10 10 10 10 10 HD165MP 60 75 100 60 60 75 75 75 100 100 Si69 4.8 6 8 4.8 4.8 6 6 6 8 8 N330 4.8 6 8 4.8 4.8 6 6 6 8 8 Vivatec700 3 30 50 3 3 30 30 30 50 50 6PPD 2 2 2 2 2 2 2 2 2 2 ZnO 2 2 2 2 2 2 2 2 2 2 SA 2 2 2 2 2 2 2 2 2 2 DPG 0.6 1 1.5 0.6 0.6 1 1 1 1.5 1.5 3,6-Bis(2-pyridyl)-1,2,4,5-tetrazine 0.7 0.6 0.6 0.8 3-Methyl-5-pyrazolone 0.5 0.5 0.5 0.5 0.8 0.8 CBS 2 2 2 2 2 2 2 2 2 2 S 1 1 1 1 1 1 1 1 1 1 The above schemes all adopt the following preparation method: Step (1) weighing the raw materials according to the weight in Table 3; Step (2) mixing the rubber for 30 seconds, adding 3-methyl-5-pyrazolone, 3,6-bis(2-pyridyl)-1,2,4,5-tetrazine, 20 parts of white carbon black HD165MP, 2 parts of silane coupling agent Si69, all vulcanization accelerators DPG and 1 part of antioxidant 6PPD, mixing and reacting at 130-150°C for 120 seconds, and debonding at 150°C to obtain material A; Step (3) The remaining raw materials except the vulcanizing agent and the vulcanization accelerator are mixed with the material A, and the mixing reaction treatment time is 140-150° C. for 120 seconds, and the rubber is discharged at 150° C. to obtain the material B; step (4) the vulcanizing agent and the vulcanization accelerator are added to the material B, mixed in an internal mixer for about 180 seconds, discharged at 110° C., and then vulcanized at 150° C. for 30 minutes to obtain a rubber composition for passenger car tires with improved cut resistance and damage resistance and reduced rolling resistance.
[0052] The rubber compositions of the comparative examples and the examples were tested for cut resistance, tear strength, tensile strength, etc. The test results are shown in Table 4.
[0053] Table 4: Test results of rubber compositions of Comparative Examples 2-1 to 2-3 and Examples 2-1 to 2-7 Test Item* Comparative Example 2-1 Comparative Example 2-2 Comparative Examples 2-3 Example 2-1 Example 2-2 Example 2-3 Embodiment 2-4 Embodiment 2-5 Embodiment 2-6 Embodiment 2-7 Mooney viscosity 100 79 75 105 100 87 78 84 85 89 Scorch time 100 89 92 117 87 90 85 79 90 82 hardness 100 101 100 99 98 99 102 98 97 97 MA100 100 99 98 89 93 87 110 97 87 95 MA300 100 96 95 78 85 76 103 90 73 88 Tensile Strength 100 97 90 99 101 102 96 90 85 88 Elongation at break 100 101 97 122 117 128 104 105 118 109 Tear strength 100 95 88 122 105 161 163 125 105 105 Hysteresis loss factor 100 128 179 111 96 129 116 119 187 140 Cutting loss 100 95 102 75 86 75 98 81 73 87 *The test results of rubber compositions are expressed in the form of indices. The calculation formula is: test item = (embodiment / comparative example 1-1) × 100.
[0054] As shown in Table 4, compared with Comparative Example 2-1, the tear strength and elongation at break of Example 2-1 increased by 22% and 22% respectively, and the cutting loss decreased by 25%, indicating that the addition of pyrazolone compounds significantly improved the tear strength, cutting loss and elongation at break of the rubber composition, and significantly improved the fatigue resistance, cutting and tearing resistance. Compared with Comparative Example 2-1, the hysteresis loss factor of Example 2-1 increased by 11%, and the heat generation and rolling resistance increased. Compared with Comparative Example 2-1, the hysteresis loss factor of Example 2-2 decreased by 4%, and compared with Example 2-1, the hysteresis loss factor of Example 2-2 decreased by 15%, that is, the addition of tetrazine compounds significantly decreased the hysteresis loss, heat generation and rolling resistance of the rubber composition. Compared with Comparative Example 2-1, the tear strength and elongation at break of Example 2-2 increased by 5% and 17% respectively, and the cutting loss decreased by 14%, indicating that the addition of tetrazine compounds on the basis of pyrazolone reduced the hysteresis loss and heat generation of the rubber composition, and significantly improved the fatigue resistance, cutting and tearing resistance.
[0055] Compared with Comparative Example 2-2, the tear strength and elongation at break of Example 2-3 are increased by 66% and 27% respectively, and the cutting loss is reduced by 20%. After increasing the amount of white carbon black filler, the addition of pyrazolone compounds still significantly improves the tear strength, cutting loss and elongation at break of the rubber composition, and the fatigue resistance, cutting resistance and tear resistance are greatly improved. Compared with Comparative Example 2-2, the hysteresis loss factor of Example 2-3 is only increased by 1%, and the hysteresis loss has a tendency to increase. Compared with Comparative Example 2-2, the hysteresis loss factor of Example 2-4 decreases by 12%, and compared with Example 2-2, the hysteresis loss factor of Example 2-5 decreases by 9%, that is, the addition of tetrazine compounds significantly reduces the hysteresis loss, heat generation and rolling resistance of the rubber composition. Compared with Example 2-2, the tear strength and elongation at break of Example 2-5 are increased by 30% and 4% respectively, and the cutting loss is reduced by 14%, indicating that by adding tetrazine compounds on the basis of pyrazolone, the hysteresis loss, heat generation and rolling resistance of the rubber composition are significantly reduced, and the anti-fatigue, cut and tear resistance are significantly improved.
[0056] In Examples 2-6 and 2-7, pyrazolone compounds and tetrazine compounds were added, and the trends of changes in physical properties were basically consistent with those in Examples 2-1 and 2-2.
[0057] The results in Table 4 show that in the formula with different contents of white carbon black filler, the addition of pyrazolone compounds significantly improves the tear strength, cutting loss and elongation at break of the rubber composition, and greatly improves the fatigue resistance, cutting and tearing resistance. The addition of tetrazine compounds on the basis of pyrazolone reduces the hysteresis loss, heat generation and rolling resistance of the rubber composition, and significantly improves the fatigue resistance, cutting and tearing resistance. Example
[0058] The raw materials used in Comparative Examples 3-1 to 3-2 and Examples 3-1 to 3-4 of the present invention are shown in the following table, all in parts by mass: Comparative Example 3-1 contains 80 parts of white carbon black, and Comparative Example 3-2 contains 60 parts of white carbon black and 20 parts of carbon black, and both comparative examples do not contain pyrazolone compounds and tetrazine compounds. Examples 3-1 and 3-2 are based on Comparative Example 3-1, and pyrazolone compounds and tetrazine compounds are added together, while Examples 3-3 and 3-4 are based on Comparative Example 3-2, and pyrazolone compounds and tetrazine compounds are added together.
[0059] Table 5: Formulations of Comparative Examples 3-1 to 3-2 and Examples 3-1 to 3-4 Material Comparative Example 3-1 Comparative Example 3-2 Example 3-1 Example 3-2 Example 3-3 Embodiment 3-4 SSBR2564S 82.5 82.5 82.5 82.5 82.5 82.5 STR20 25 25 25 25 25 25 BR9000 15 15 15 15 15 15 N234 20 20 20 HD165MP 80 60 80 80 60 60 Si69 6.4 4.8 6.4 6.4 4.8 4.8 N330 6.4 4.8 6.4 6.4 4.8 4.8 Vivatec700 13.5 13.5 13.5 13.5 13.5 13.5 6PPD 2.1 2.1 2.1 2.1 2.1 2.1 Antilux111 1.5 1.5 1.5 1.5 1.5 1.5 TMQ 1 1 1 1 1 1 SAD 2 2 2 2 2 2 DPG 1 1 1 1 1 1 ZnO 2 2 2 2 2 2 3,6-Bis(2-pyridyl)-1,2,4,5-tetrazine 0.7 0.7 3-Methyl-5-pyrazolone 0.5 0.5 0.5 0.5 CBS 2.3 2.3 2.3 2.3 2.3 2.3 S 1 1 1 1 1 1 The above schemes all adopt the following preparation method: Step (1) weigh the raw materials according to the weight in Table 3; Step (2) mix the rubber for 30 seconds, add 3-methyl-5-pyrazolone, 3,6-bis(2-pyridyl)-1,2,4,5-tetrazine, 20 parts of white carbon black HD165MP, 2 parts of silane coupling agent Si69, all vulcanization accelerators DPG, and 1 part of antioxidant 6PPD, mix and react at 130-150°C for 120 seconds, and remove the rubber at 150°C to obtain material A; Step (3) The remaining raw materials except the vulcanizing agent and the vulcanization accelerator are mixed with the material A, and the mixing reaction treatment time is 140-150° C. for 120 seconds, and the rubber is discharged at 150° C. to obtain the material B; step (4) the vulcanizing agent and the vulcanization accelerator are added to the material B, mixed in an internal mixer for about 180 seconds, discharged at 110° C., and then vulcanized at 150° C. for 30 minutes to obtain a rubber composition for passenger car tires with improved cut resistance and damage resistance and reduced rolling resistance.
[0060] The rubber compositions of the comparative example and the examples were tested for cut resistance, tear strength, tensile strength, etc. The test results are shown in Table 6.
[0061] Table 6: Test results of rubber compositions of Comparative Examples 3-1 to 3-2 and Examples 3-1 to 3-4 Test Item* Comparative Example 3-1 Comparative Example 3-2 Example 3-1 Example 3-2 Example 3-3 Embodiment 3-4 Mooney viscosity 100 118 112 121 129 130 Scorch time 100 140 142 116 130 113 hardness 100 93 96 98 94 92 MA100 100 92 86 103 89 83 MA300 100 95 88 108 87 79 Tensile Strength 100 100 100 102 97 100 Elongation at break 100 103 111 104 109 118 Tear strength 100 99 103 105 109 112 Hysteresis loss factor 100 102 95 90 98 96 Cutting loss 100 98 95 97 78 70 *The test results of rubber compositions are expressed in the form of indices. The calculation formula is: test item = (embodiment / comparative example 1-1) × 100.
[0062] As shown in Table 6, compared with Comparative Example 3-1, the tear strength and elongation at break of Example 3-1 increased by 3% and 11% respectively, and the cutting loss decreased by 5%, indicating that the addition of pyrazolone compounds significantly improved the tear strength, cutting loss and elongation at break of the rubber composition, and improved the fatigue resistance, cutting and tearing resistance. Compared with Comparative Example 3-1, the hysteresis loss factor of Example 3-1 decreased by 5%, and the heat generation and rolling resistance decreased. Compared with Comparative Example 3-1, the hysteresis loss factor of Example 3-2 decreased by 10%, and compared with Example 3-1, the hysteresis loss factor of Example 3-2 decreased by 5%, that is, the addition of tetrazine compounds further decreased the hysteresis loss, heat generation and rolling resistance of the rubber composition. Compared with Comparative Example 3-1, the tear strength and elongation at break of Example 3-2 increased by 5% and 4% respectively, and the cutting loss decreased by 3%, indicating that the addition of tetrazine compounds on the basis of pyrazolone reduced the hysteresis loss, heat generation and rolling resistance of the rubber composition, and significantly improved the fatigue resistance, cutting and tearing resistance.
[0063] As shown in Table 6, compared with Comparative Example 3-2, the tear strength and elongation at break of Example 3-3 are increased by 10% and 6%, respectively, and the cutting loss is reduced by 20%, indicating that the addition of pyrazolone compounds, the tear strength, cutting loss, and elongation at break of the rubber composition are significantly improved, and the fatigue resistance, cutting and tearing resistance are improved. Compared with Comparative Example 3-2, the hysteresis loss factor of Example 3-3 decreases by 4%, and the heat generation and rolling resistance decrease. Compared with Comparative Example 3-2, the hysteresis loss factor of Example 3-4 decreases by 6%, that is, the addition of tetrazine compounds further decreases the hysteresis loss, heat generation, and rolling resistance of the rubber composition. Compared with Comparative Example 3-2, the tear strength and elongation at break of Example 3-4 are increased by 13% and 15%, respectively, and the cutting loss is reduced by 28%, indicating that the addition of tetrazine compounds on the basis of pyrazolone, the hysteresis loss, heat generation, and rolling resistance of the rubber composition decrease, and the fatigue resistance, cutting and tearing resistance are significantly improved.
[0064] The results in Table 6 show that in the formula system where the filler is white carbon black or white carbon black and carbon black are used in combination, the addition of pyrazolone compounds still significantly improves the tear strength, cutting loss, and elongation at break of the rubber composition, and improves the fatigue resistance, cutting resistance, and tear resistance. When tetrazine compounds are added to pyrazolone, the hysteresis loss, heat generation, and rolling resistance of the rubber composition decrease, and the fatigue resistance, cutting resistance, and tear resistance are significantly improved.
[0065] The above examples show that the pyrazolone compound significantly improves the tear strength and elongation at break of the rubber composition, significantly reduces the cutting loss, and can improve the fatigue resistance, cutting and tearing resistance of the rubber composition. The pyrazolone compound may have an effect on the hysteresis loss, heat generation and rolling resistance of the rubber composition. When the tetrazine compound is added alone, the hysteresis loss, heat generation and rolling resistance of the rubber composition are significantly reduced. When the pyrazolone compound and the tetrazine compound are used together, the hysteresis loss, heat generation and rolling resistance of the rubber composition are reduced, and the fatigue resistance, cutting and tearing resistance are significantly improved.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composition for cutting resistance and fatigue resistance of passenger car tires, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of diene rubber, 0.2-1.5 parts of pyrazolone compounds, 0-1.5 parts of tetrazine compounds, 20-150 parts of reinforcing fillers, 2-20 parts of silane coupling agents, vulcanization accelerators, vulcanizing agents, antioxidants, vulcanization activators, resins and plasticizers; The structure of the tetrazine compound is: (1) Wherein X1 and X2 represent a heterocyclic group which may have a substituent; The structure of the pyrazolone compound is: (2) (3) Among them, R1, R2, R3, and R4 are the same or different, representing a hydrogen atom, an alkyl group, an aralkyl group, an aryl group or a heterocyclic group; R3 and R4 can be connected to form an alkylene group, and any two of R2, R3 and R4 can be connected together to form an alkylene group; R5, R7, R8 are the same or different, representing a hydrogen atom, an alkyl group, an aralkyl group, an aryl group or a heterocyclic group; R6 represents an alkyl group, an aralkyl group, an aryl group or a heterocyclic group, and each of these groups can have one or more substituents.
2. The composition for cutting resistance and fatigue resistance of passenger car tires according to claim 1, characterized in that: The diene rubber is any one or more combinations of modified or unmodified natural rubber, polyisoprene rubber, polybutadiene rubber, butadiene rubber, styrene-butadiene copolymer rubber, ethylene-propylene-diene monomer copolymer, styrene-isoprene-styrene terblock copolymer rubber, and styrene-butadiene-styrene terblock copolymer rubber.
3. The composition for cutting resistance and fatigue resistance of passenger car tires according to claim 2, characterized in that: The diene rubber is any one or more combinations of modified or unmodified styrene-butadiene copolymer rubber and polybutadiene rubber, and the amount of the styrene-butadiene copolymer rubber and polybutadiene rubber is 50-100 parts.
4. The composition for cutting resistance and fatigue resistance of passenger car tires according to claim 2, characterized in that: The diene rubber is a combination of any one or more of modified or unmodified natural rubber and polyisoprene rubber, and the amount of the natural rubber and polyisoprene rubber is 0-50 parts.
5. The composition for cutting resistance and fatigue resistance of passenger car tires according to claim 1, characterized in that: The pyrazolone compound is any one or more of 3-methyl-5-pyrazolone, 3-phenyl-5-pyrazolone, 3-ethyl-5-pyrazolone, 3-propyl-5-pyrazolone and 3-butyl-5-pyrazolone, and the amount of the pyrazolone compound is 0.3-1.2 parts.
6. The composition for cut resistance and fatigue resistance of passenger car tires according to claim 1, characterized in that: The tetrazine compound is any one or more of 3,6-bis(2-pyridyl)-1,2,4,5-tetrazine, 3,6-bis(3-pyridyl)-1,2,4,5-tetrazine, and 3,6-bis(4-pyridyl)-1,2,4,5-tetrazine. The amount of the tetrazine compound is 0-1.2 parts.
7. The composition for cutting resistance and fatigue resistance of passenger car tires according to claim 1, characterized in that: The reinforcing filler is any one or more of modified or unmodified carbon black, acetylene black, white carbon black, carbon nanotubes, graphite, and graphene, wherein the amount of white carbon black in the reinforcing filler is 50-150 parts, and the amount of carbon black is 0-50 parts; The silane coupling agent is a combination of any one or more of bis-[3-(triethoxysilyl)propyl]-tetrasulfide, bis-[3-(triethoxysilyl)propyl]-disulfide, 3-octanoylthio-1-propyltriethoxysilane, γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane) and mercaptoalkoxy-ethoxy or methoxysilane, and the amount of the silane coupling agent is 3-18 parts.
8. A method for preparing a composition for passenger car tires that is resistant to cutting and fatigue, for preparing the composition for passenger car tires that is resistant to cutting and fatigue according to claim 1, characterized in that: The following steps are involved: Step (1) weighing various raw materials: the raw materials include diene rubber, pyrazolone compound, tetrazine compound reinforcing filler, silane coupling agent, vulcanization accelerator, vulcanizing agent, antioxidant, vulcanization activator, resin and plasticizer; Step (2) mixing diene rubber, pyrazolone compound, tetrazine compound, antioxidant, reinforcing filler, silane coupling agent, and vulcanization accelerator diphenylguanidine, and performing a mixing reaction at 120-180° C. for 60-300 seconds, and cooling the mixture to obtain material A; Step (3) mixing the remaining raw materials except the vulcanizing agent and the vulcanization accelerator with material A, and performing a mixing reaction at 120-180° C. for 60-300 seconds, and then cooling to obtain material B; Step (4) adding a vulcanizing agent and a vulcanization accelerator to material B, mixing and discharging the material, and then performing a vulcanization reaction to obtain a rubber composition for improving cut resistance and damage resistance and reducing rolling resistance.
9. The method for preparing a composition for cut resistance and fatigue resistance of passenger car tires according to claim 8, characterized in that: The mixing reaction time in step (2) and step (3) is 2-10 minutes, the discharge temperature is 120-180° C., the vulcanization temperature is 130-180° C., and the vulcanization time is 10-200 minutes.
10. A passenger car tire, characterized in that: The tire is prepared by using the composition for cutting resistance and fatigue resistance of passenger car tires as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Additive for imparting low heat build-up to rubber component
CN108026332A
Rubber composition, rubber material, use of same and additive
CN112533991A
Tear-resistant and cutting-resistant rubber track composition and preparation method thereof
CN116265516A
Rubber composition with self-repairing capability by utilizing dynamic cross-linked bonds as well as preparation method and application of rubber composition
CN118374066A
Tire rubber composition, and tire
JP2020097696A