Quick-dormancy reserve type lithium ion battery, preparation method thereof and composite electrolyte adopted by quick-dormancy reserve type lithium ion battery
By using a composite electrolyte with lithium salt, electrolyte additive and low boiling point solvent, combined with the method of removing solvent in vacuum, the problem of complex production process and long activation time of lithium-ion battery is solved, rapid dormant and activation are achieved, and the battery is improved The specific energy and power performance simplifies the manufacturing process.
Patent Information
- Application Number
- CN202310622221.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The production process of lithium ion storage batteries is complex, the activation time is long, and it is difficult to meet the actual application needs. The existing technology has problems of complex operation and insufficient performance.
The composite electrolyte containing lithium salt, electrolyte additives and low boiling point solvents is used to sleep the battery by vacuum removal, simplifying the preparation process of lithium-ion batteries, and achieving rapid dormant and activation.
It realizes rapid dormant and activation of lithium-ion batteries, reduces production costs, improves specific energy and power performance, simplifies the manufacturing process, and is suitable for large-scale production.
Smart Images

Figure CN119069769A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of activated lithium reserve batteries, in particular to a fast dormant reserve lithium ion battery and a preparation method and a composite electrolyte used therein, which shortens the activation time of the lithium reserve battery and is used in a secondary battery system and a primary battery system. Background Art
[0002] Compared with traditional zinc-silver, aluminum-silver, thermal batteries and other traditional reserve batteries, lithium-ion reserve batteries have the characteristics of high specific energy, small volume, excellent power performance, and strong environmental applicability. They are currently a hot research topic for new reserve batteries. They can be used in ammunition weapons such as torpedoes and rocket launchers, significantly improving the combat capability of weapons and equipment.
[0003] Looking at the current status of lithium-ion reserve battery technology development at home and abroad, there are two main methods for preparing reserve lithium-ion batteries, namely, preparing de-lithiated positive electrode materials and then producing them through conventional lithium-ion battery preparation methods; and first preparing de-lithiated positive electrode plates and then reassembling lithium-ion batteries. Using heat-sensitive electrolyte solvent materials, etc., the battery activation time is long, which is difficult to meet application requirements; using detached positive electrode materials, dormancy and activation methods all have problems such as complex operations, which makes it difficult to promote the practical application of reserve lithium-ion batteries. For example, CN113937366A is a method and application for shortening the activation time of lithium reserve batteries, which mainly prepares detached positive electrode plates first, then reassembles dry batteries, realizes the storage of lithium-ion batteries, and then quickly activates them through commercial electrolytes. CN109755656B is a new type of "self-activating" lithium-ion secondary reserve battery and its preparation method, which uses heat-sensitive electrolyte solvent materials and realizes the storage of lithium-ion batteries through the characteristics of low ionic conductivity at low temperatures. The CN202423481U fully sealed automatic activation type lithium-sulfur battery pack adopts a lithium-sulfur battery system and a fully sealed structure to prepare a reserve type lithium-sulfur battery pack.
[0004] Existing lithium-ion reserve batteries have a complicated manufacturing process. CN113937366A needs to be made into a conventional lithium-ion battery first, and then the positive electrode sheet is disassembled and the battery is reassembled after charging and discharging, which is not conducive to mass production. CN109755656B uses a thermosensitive electrolyte and low ion conductivity under low temperature conditions to achieve battery dormancy. It needs to be stored under low temperature conditions, which is not conducive to practical application. CN202423481U uses a lithium-sulfur battery, which has poor volume-to-energy and power performance and is difficult to meet actual use needs. Summary of the invention
[0005] The technical problem to be solved by the present invention is that, in view of the complex manufacturing process of lithium ion reserve batteries, a fast dormant reserve lithium ion battery and a preparation method and a composite electrolyte are proposed. The composite electrolyte comprising lithium salt, electrolyte additive and low boiling point solvent is used to prepare the battery according to a conventional lithium ion battery preparation method. After the battery is fully charged, the solvent is removed by vacuum to put the battery into dormancy and realize storage.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a composite electrolyte, comprising a low-boiling-point solvent with a boiling point lower than 100°C, a lithium salt and an additive, wherein the concentration of the lithium salt is lower than 1.2 mol / L, and the mass percentage concentration of the additive is lower than 10%;
[0007] The solvent is one or more low-boiling-point solvents selected from ethers, alkylene oxides, esters, ketones, carbon tetrachloride, and tetrahydrofuran, with a boiling point lower than 100°C;
[0008] The lithium salt is one or more of lithium hexafluorophosphate, bis(fluorosulfonyl)imide lithium salt, lithium difluorophosphate, lithium difluorooxalatoborate, and lithium tetrafluoroborate;
[0009] The additive is one or more of vinylene carbonate, vinyl sulfate, 1,3-propane sultone, fluoroethylene carbonate, 1,3,6-hexanetrinitrile, succinonitrile and adiponitrile.
[0010] A method for manufacturing a fast dormant lithium-ion battery comprises the following steps:
[0011] 1) Battery assembly: Lithium-ion battery electrode groups are made by winding or lamination and then packaged;
[0012] 2) Pole group drying: The assembled battery is dried at high temperature in a vacuum;
[0013] 3) Liquid injection: After drying, the composite electrolyte prepared above is used for liquid injection under a temperature-controlled environment;
[0014] 4) Infiltration: In a temperature-controlled environment, place the battery after injection to stand until the inside is fully infiltrated;
[0015] 5) First charge and discharge: The lithium-ion battery after injection and immersion is charged and discharged using a charge and discharge process, and finally the battery is charged to a fully charged state.
[0016] 6) Dormancy: vacuum remove the solvent by increasing the temperature in stages until the battery weight stops decreasing.
[0017] The temperature of the temperature-controlled environment in step 3) and step 4) is related to the boiling point of the solvent of the low-boiling-point composite electrolyte used, and the temperature environment is 0 to 20 degrees Celsius lower than the boiling point of the solvent.
[0018] The infiltration time of step 4) is ≥ 12 hours.
[0019] In step 5), the charge and discharge current is 0.01C to 5C.
[0020] The temperature range of vacuum removal of solvent in step 6) is room temperature to 100° C., and the vacuum degree is ≤-95 kPa.
[0021] The fast dormant reserve lithium ion battery is manufactured by the above manufacturing method.
[0022] The fast dormant reserve lithium-ion battery comprises a lithium-ion secondary battery system of lithium iron phosphate, lithium iron manganese phosphate, lithium-rich manganese base, lithium vanadium phosphate, lithium cobalt oxide, ternary lithium positive electrode with metallic lithium, graphite, silicon-containing negative electrode, lithium titanate, and lithium niobium titanate negative electrode.
[0023] The beneficial effects of the present invention are:
[0024] 1. The lithium-ion battery electrolyte of the present invention constructs a storage-resistant electrochemical system through a high-stability electrolyte additive, realizes rapid truncation of lithium ion channels to achieve battery dormancy through a rapid solvent removal method, and can reactivate the battery through a low-viscosity electrolyte. It has the advantages of high specific energy, simple production, long storage time, and rapid activation.
[0025] 2. The low-boiling-point and easy-to-remove-solvent electrolyte of the present invention can meet the requirements of battery film formation, charge and discharge during the battery manufacturing stage. After the formation is completed, the solvent can be quickly removed by vacuuming. After the solvent is removed, the lithium ion transmission channel inside the battery is cut off, meeting the dormancy requirements of the reserve lithium ion battery. The production cost of the reserve lithium ion battery is significantly reduced, and it has high practical value. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a 5C rate discharge curve of the dormant lithium-ion battery of Example 3 of the present invention after reactivation. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments, and all other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making creative work are within the scope of protection of the present invention.
[0028] The composite electrolyte of the present invention comprises a low-boiling-point solvent having a boiling point lower than 100° C., a lithium salt and an additive, wherein the lithium salt concentration is lower than 1.2 mol / L, and the mass percentage concentration of the additive is lower than 10%;
[0029] The solvent is one or more low-boiling-point solvents selected from ethers, alkylene oxides, esters, ketones, carbon tetrachloride, and tetrahydrofuran, with a boiling point lower than 100°C;
[0030] The lithium salt is one or more of lithium hexafluorophosphate, bis(fluorosulfonyl)imide lithium salt, lithium difluorophosphate, lithium difluorooxalatoborate, and lithium tetrafluoroborate;
[0031] The additive is one or more of vinylene carbonate (VC), diethylene sulfate (DTD), 1,3-propane sultone (PS), fluoroethylene carbonate (FEC), 1,3,6-hexanetrinitrile (HTCN), succinonitrile (SN), and adiponitrile (ADN).
[0032] A method for manufacturing a fast dormant lithium-ion battery comprises the following steps:
[0033] 1) Battery assembly: Lithium-ion battery electrode groups are made by winding or lamination and then packaged;
[0034] 2) Pole group drying: The assembled battery is dried at high temperature in a vacuum;
[0035] 3) Liquid injection: After drying, the composite electrolyte prepared above is used for liquid injection under a temperature-controlled environment;
[0036] 4) Infiltration: In a temperature-controlled environment, place the battery after injection to stand until the inside is fully infiltrated;
[0037] 5) First charge and discharge: The lithium-ion battery after injection and immersion is charged and discharged using a charge and discharge process, and finally the battery is charged to a fully charged state.
[0038] 6) Dormancy: vacuum remove the solvent by increasing the temperature in stages until the battery weight stops decreasing.
[0039] The temperature of the temperature-controlled environment in step 3) and step 4) is related to the boiling point of the solvent of the low-boiling-point composite electrolyte used, and the temperature environment is 0 to 20 degrees Celsius lower than the boiling point of the solvent.
[0040] The infiltration time of step 4) is ≥ 12 hours.
[0041] In step 5), the charge and discharge current is 0.01C to 5C.
[0042] The temperature range of vacuum removal of solvent in step 6) is room temperature to 100° C., and the vacuum degree is ≤-95 kPa.
[0043] The fast dormant reserve lithium ion battery is manufactured by the above manufacturing method.
[0044] The fast dormant reserve lithium-ion battery comprises a lithium-ion secondary battery system of lithium iron phosphate, lithium iron manganese phosphate, lithium-rich manganese base, lithium vanadium phosphate, lithium cobalt oxide, ternary lithium positive electrode with metallic lithium, graphite, silicon-containing negative electrode, lithium titanate, and lithium niobium titanate negative electrode.
[0045] The reserve lithium ion battery prepared by the present invention has the advantages of high specific energy and good power performance, and has the potential to replace the existing reserve batteries. In order to improve the manufacturing process of the reserve lithium ion battery. According to the existing manufacturing process of lithium ion batteries, the present invention adopts an electrolyte with a low boiling point solvent to manufacture the battery, and then realizes the dormancy of the battery by quickly removing the solvent, thereby realizing the storage of lithium ion batteries.
[0046] The technical solution of the present invention is described in detail below through embodiments, but the protection scope of the present invention is not limited to the embodiments.
[0047] The method for rapidly dormant reserve lithium ion batteries of the present invention comprises a pre-prepared low-boiling-point solvent composite electrolyte.
[0048] Step 1) Battery assembly: Use a coating amount of 40 mg / cm 2 The lithium cobalt oxide positive electrode is matched with a 50-micron thick metal lithium negative electrode to stack and package the batteries. The nominal capacity of the battery is 10Ah.
[0049] Step 2) Drying of the electrode group: The assembled battery is subjected to high-temperature vacuum drying, the drying temperature is 90°C, the vacuum degree is ≤-95kPa, and the drying time is ≥12h.
[0050] Step 3) The electrolyte configuration is shown in the following table:
[0051] Table 1. Examples of electrolytes with different ratios
[0052]
[0053] The electrolytes in the above proportions are mixed and stirred evenly, and allowed to stand for 1 hour before use.
[0054] Liquid injection: After drying and testing the electrode group for qualified moisture, use the composite electrolyte prepared with the above-mentioned low boiling point solvent to inject liquid at 25℃±3℃;
[0055] Step 4) Infiltration: The battery after injection is left to stand at 25°C ± 3°C for about 24 hours;
[0056] Step 5) First charge and discharge: Use 0.3C constant current and constant voltage to 4.4V, cut-off current 0.05C, and fully charge the battery;
[0057] Step 6) Sleep: Place the battery in a vacuum box at 25°C ± 3°C and evacuate for 12 hours. When the vacuum degree is ≤-99 kPa, slowly increase the oven temperature to the boiling point of the mixed solvent and continue evacuating for 24 hours.
[0058] Table 2. Comparison of the above batteries before and after sleep
[0059] project Example 1 Example 2 Example 3 Example 4 Internal resistance before sleep 4mΩ 4.2mΩ 3.9mΩ 4.4mΩ Voltage before sleep 4.37V 4.35V 4.36V 4.34V Internal resistance after sleep ∞ ∞ ∞ ∞ Voltage after sleep 0V 0V 0V 0V
[0060] like Figure 1 As shown, the present invention uses an electrolyte system compounded with a low-boiling point solvent to quickly remove the solvent after the battery is fully charged, thereby blocking the lithium ion transmission path inside the battery and achieving lithium ion battery hibernation. This method is simple to manufacture the battery and is conducive to promoting the engineering process of reserve lithium ion batteries.
[0061] The embodiments described above are only used to illustrate the technical ideas and features of the present invention, and their purpose is to enable those skilled in the art to understand the contents of the present invention and implement them accordingly. The patent scope of the present invention cannot be limited only by this embodiment, that is, any equivalent changes or modifications made to the spirit disclosed by the present invention still fall within the patent scope of the present invention.
Claims
1. A composite electrolyte, characterized in that: Including low boiling point solvents with a boiling point below 100°C, lithium salts and additives, the lithium salt concentration is lower than 1.2 mol / L, and the mass percentage concentration of the additives is lower than 10%; The solvent is one or more low-boiling-point solvents selected from ethers, alkylene oxides, esters, ketones, carbon tetrachloride, and tetrahydrofuran, with a boiling point lower than 100°C; The lithium salt is one or more of lithium hexafluorophosphate, bis(fluorosulfonyl)imide lithium salt, lithium difluorophosphate, lithium difluorooxalatoborate, and lithium tetrafluoroborate; The additive is one or more of vinylene carbonate, vinyl sulfate, 1,3-propane sultone, fluoroethylene carbonate, 1,3,6-hexanetrinitrile, succinonitrile and adiponitrile.
2. A method for manufacturing a fast dormant reserve lithium-ion battery, characterized in that: The steps include: 1) Battery assembly: Lithium-ion battery electrode groups are made by winding or lamination and then packaged; 2) Pole group drying: The assembled battery is dried at high temperature in a vacuum; 3) Liquid injection: After drying, the composite electrolyte prepared in claim 1 is used for liquid injection under a temperature-controlled environment; 4) Infiltration: In a temperature-controlled environment, place the battery after injection to stand until the inside is fully infiltrated; 5) First charge and discharge: The lithium-ion battery after injection and immersion is charged and discharged using a charge and discharge process, and finally the battery is charged to a fully charged state. 6) Dormancy: vacuum remove the solvent by increasing the temperature in stages until the battery weight stops decreasing.
3. The method for manufacturing a fast dormant reserve lithium-ion battery according to claim 2, characterized in that: The temperature of the temperature-controlled environment in step 3) and step 4) is related to the boiling point of the solvent of the low-boiling-point composite electrolyte used, and the temperature environment is 0 to 20 degrees Celsius lower than the boiling point of the solvent.
4. The method for manufacturing a fast dormant reserve lithium-ion battery according to claim 2, characterized in that: The infiltration time of step 4) is ≥ 12 hours.
5. The method for manufacturing a fast dormant reserve lithium-ion battery according to claim 2, characterized in that: In step 5), the charge and discharge current is 0.01C to 5C.
6. The method for manufacturing a fast dormant reserve lithium-ion battery according to claim 2, characterized in that: The temperature range of vacuum removal of solvent in step 6) is room temperature to 100° C., and the vacuum degree is ≤-95 kPa.
7. A fast dormant reserve lithium-ion battery made by the method according to any one of claims 2 to 6.
8. The fast dormant reserve lithium-ion battery according to claim 1, characterized in that: Lithium-ion secondary battery systems including lithium iron phosphate, lithium iron manganese phosphate, lithium-rich manganese-based, lithium vanadium phosphate, lithium cobalt oxide, ternary lithium positive electrode with metallic lithium, graphite, silicon-containing negative electrode, lithium titanate, and lithium niobium titanate negative electrode.
Citation Information
Patent Citations
A novel self-activated lithium-ion secondary storage battery and its preparation method
CN109755656B
Method for shortening activation time of lithium reserve battery and application