Combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals and application of combined inhibitor
Through the combined inhibitor of water glass, iminodisuccinic acid and carboxymethylcellulose, the problem of separation of fluorite and calcium-containing ganglite minerals was solved, the flotation efficiency and grade were improved, the dosage of the agent was reduced, and the Environmental protection and low cost advantages.
Patent Information
- Application Number
- CN202411227776.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The prior art is difficult to effectively separate fluorite and calcium-containing ganglite minerals. Traditional water glass inhibitors have weak selectivity and high usage, resulting in low flotation and separation efficiency of fluorite ore. With the depletion of fluorite ore, single inhibition is achieved. The effect of the agent is getting worse and worse.
Using a combination inhibitor of water glass, iminodisuccinic acid and carboxymethyl cellulose, an aqueous solution is prepared by heating and strong stirring, for flotation separation of fluorite and calcium-containing ganglite minerals, using iminodisuccinic acid The dispersion effect of polar groups and carboxymethyl cellulose achieves selective adsorption and dispersion of calcareous ganglite minerals.
The flotation separation efficiency between fluorite and calcium-containing ganglite minerals is improved, the amount of flotation agent is reduced, and high-grade fluorite concentrate is obtained. The combination inhibitor is environmentally friendly, low-cost and easy to operate.
Smart Images

Figure CN119076233A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals and application thereof, belonging to the technical field of mineral processing flotation. Background Art
[0002] Fluorite is an important non-metallic strategic mineral resource and one of the important sources of elemental fluorine. Fluorite in nature often coexists with calcium-containing gangue minerals such as calcite and dolomite. Flotation is the most important and efficient method for processing and enriching fluorite ore. Fluorite ore and calcium-containing gangue minerals such as calcite and dolomite are all calcareous minerals. They have similar surface chemical properties, solution chemical properties and the same calcium ion active sites. When flotated with traditional fatty acid collectors, their floatability is similar and it is difficult to separate them by flotation. Therefore, the development, selection and application of efficient flotation separation inhibitors are crucial.
[0003] At present, the most widely used inhibitor in the flotation separation industry of fluorite and calcium-containing gangue minerals is still the traditional inhibitor water glass. In the flotation process, the amount of water glass used is large, and the selective inhibition effect is poor. Adding a large amount of water glass will also make the tailings highly dispersed, difficult to settle, and difficult to treat the ore dressing wastewater. At the same time, with the continuous development and utilization of fluorite, fluorite is becoming more and more poor, fine, and mixed. The effect of a single water glass inhibitor is getting lower and lower, and it is difficult to achieve efficient flotation separation of fluorite.
[0004] Iminodisuccinic acid is a new type of environmentally friendly chelating agent with good water solubility and easy biodegradation. The hydrophilic carboxyl group in its molecular structure can be adsorbed on the surface of calcium-containing minerals and can also play an inhibitory role. Carboxymethyl cellulose has a wide and abundant source, is soluble in water, and is often used as an inhibitor in mineral processing. Therefore, the development of green, low-cost and efficient combined inhibitors of calcium-containing gangue minerals in the efficient flotation separation of fluorite ore is the future development trend of fluorite ore processing, which is of great significance to improving the utilization rate of fluorite ore resources in my country. Summary of the invention
[0005] In order to solve the problem of difficulty in flotation separation of fluorite and calcareous gangue minerals such as calcite, apatite and dolomite in the flotation process of fluorite, the purpose of the present invention is to provide a combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals and its application, which is used to solve the problem of difficulty in flotation separation of fluorite and calcareous gangue minerals in the flotation process of fluorite.
[0006] The combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals of the present invention comprises water glass, iminodisuccinic acid and carboxymethyl cellulose.
[0007] Preferably, the mass percentage of water glass in the combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals is 60% to 75%, the mass percentage of iminodisuccinic acid is 15% to 30%, the mass percentage of carboxymethyl cellulose is 10% to 25%, and the total mass percentage of water glass, iminodisuccinic acid and carboxymethyl cellulose is 100%.
[0008] The present invention also provides an application of a combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals in the flotation separation of fluorite and calcareous gangue minerals.
[0009] Preferably, fluorite concentrate and fluorite tailings are obtained from fluorite ore by flotation separation through a process flow of one roughing selection, seven cleaning selections and two scavenging selections.
[0010] Preferably, the combined inhibitor is added in the first roughing and the seventh fine cleaning, and is not added in other processes.
[0011] Preferably, the amount of combined inhibitor added in the roughing process is 450-750 g / t; in the seven concentration processes, the amount of combined inhibitor added in concentration I and concentration II is 150-250 g / t, the amount of combined inhibitor added in concentration III, concentration IV and concentration V is 50-84 g / t, and the amount of combined inhibitor added in concentration VI and concentration VII is 16-28 g / t.
[0012] Preferably, the combined inhibitor is first dissolved in ultrapure water when used. The specific preparation method is: water glass, iminodisuccinic acid and carboxymethyl cellulose are added to ultrapure water at the same time, and heated and strongly stirred to obtain the inhibitor aqueous solution.
[0013] Preferably, the total mass concentration of water glass, iminodisuccinic acid and carboxymethyl cellulose in the inhibitor aqueous solution is 15% to 20%, and the concentration of the combined inhibitor is diluted to 1% to 2% during flotation dosing.
[0014] Preferably, the heating temperature is 60° C. to 70° C., and the stirring intensity is 1200 to 1500 r / min.
[0015] Preferably, the specific process flow of flotation separation is as follows:
[0016] (1) Grind the ore sample and adjust the slurry to the required slurry concentration and pH value.
[0017] (2) Fluorite roughing: adding a combined depressant to the slurry obtained in step (1), stirring, adding a collector, stirring, and flotation to obtain a fluorite rough concentrate and a calcium-containing gangue tailing.
[0018] (3) Fluorite scavenging: The calcium gangue tailings obtained in step (2) are subjected to fluorite scavenging, scavenging I, adding a collector, stirring, and flotation; scavenging II, adding a collector, stirring, and flotation to obtain the final fluorite tailings.
[0019] (4) Fluorite concentration: The rough concentrate obtained in step (2) is subjected to fluorite concentration. The steps of concentration I to concentration VII are as follows: adding a combined depressant, stirring, flotation, and obtaining the final fluorite concentrate.
[0020] Preferably, in step (1), the grinding fineness satisfies -0.074 mm, accounting for 70-80%.
[0021] Preferably, in step (1), the slurry concentration is 25-35%, the slurry pH is 9-11, the adjusting agent is one or a combination of two of sodium hydroxide and sodium carbonate in any proportion, and the slurry adjustment time is 2-3 minutes.
[0022] Preferably, in the step (2) of fluorite roughing, the amount of combined depressant added is 450-750 g / t, and the amount of collector added is 500-750 g / t; the stirring time is 2-3 min, and the flotation time is 4-5 min.
[0023] Preferably, in step (3), the amount of collector added in scavenging I is 180-250 g / t; the amount of collector added in scavenging II is 60-150 g / t; the stirring time of scavenging I and scavenging II is 2-3 min, the flotation time of scavenging I is 3-4 min, and the flotation time of scavenging II is 2.5-3.5 min.
[0024] Preferably, in step (4), the amount of combined depressant added to Concentrated I and Concentrated II is 150-250 g / t, the stirring time is 2-3 min, and the flotation time is 2-3 min; the amount of combined depressant added to Concentrated III, Concentrated IV and Concentrated V is 50-84 g / t, the stirring time is 2-3 min, and the flotation time is 2-3 min; the amount of combined depressant added to Concentrated VI and Concentrated VII is 16-28 g / t, the stirring time is 2-3 min, and the flotation time is 2-3 min.
[0025] The collector used in the flotation separation process is a common collector in flotation separation.
[0026] Principle of the present invention: Water glass is a commonly used flotation depressant for calcium-containing gangue minerals, but it is subject to the constraints of weak selectivity, acidification treatment, and difficulty in treating ore dressing wastewater during use, so it has limitations in actual production; the molecular formula of iminodisuccinic acid is C8H 11 O8N, the structural formula is It contains a large number of polar carboxyl groups, which can selectively adsorb on the surface of calcium-containing gangue minerals and inhibit the gangue minerals; carboxymethyl cellulose is a soluble natural polymer compound, which can be used as an inhibitor of calcium-containing gangue minerals in the slurry solution, and it can also be used as a dispersant to disperse the slurry, which helps the adsorption of flotation reagents on the mineral surface. A new compound is generated by heating and mixing iminodisuccinic acid, water glass and carboxymethyl cellulose. The water glass dispersed slurry particles are more easily adsorbed by the reagent, iminodisuccinic acid has good selectivity, and the four carboxyl groups in the molecular structure can be stably adsorbed on the calcium sites of calcium-containing gangue minerals. Carboxymethyl cellulose makes the mineral particles more hydrophilic, and the new compound has a synergistic inhibitory effect on the surface of calcium-containing gangue minerals.
[0027] Beneficial Effects of the Invention
[0028] (1) The present invention proposes for the first time to use a combination of an inorganic inhibitor, water glass, an organic small molecule inhibitor, iminodisuccinic acid, and an organic macromolecule inhibitor, carboxymethyl cellulose, as a combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals. Its application in fluorite flotation has not been reported yet.
[0029] (2) The combined inhibition in the present invention is applied to fluorite flotation to achieve efficient flotation separation of fluorite and calcium-containing gangue minerals, thereby obtaining high-grade fluorite concentrate, reducing the amount of flotation reagents used, and improving separation efficiency.
[0030] (3) The components of the combined depressant in the present invention are widely available, have good environmental properties, are convenient to configure, and are easy to operate and implement, and can effectively improve the flotation separation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Flow chart of fluorite flotation process for embodiments and comparative examples. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0033] Example 1
[0034] In this embodiment, the mass percentages of water glass, iminodisuccinic acid and carboxymethyl cellulose in the combined inhibition components are 70%, 15% and 15%, respectively, and the collector is a sodium oleate aqueous solution.
[0035] A fluorite mine in Hunan is a calcite-type fluorite paragenesis mine. The fluorite content in the original ore is 31.43%. The gangue minerals mainly include calcite, quartz and feldspar, etc. The calcite content is 20.46%, and the SiO2 content is 17.32%. The flotation process adopts a closed-circuit test process of one coarse, seven fine, and two sweeps, and the intermediate ore is returned in sequence. The flotation separation process of this embodiment is as follows: Figure 1 The flotation results are shown in Table 1. The specific steps and experimental conditions are as follows:
[0036] (1) Grind the raw ore to a grinding fineness of -0.074 mm, accounting for 75%, adjust the pulp concentration to 25%, and use pH adjuster sodium carbonate to adjust the pulp pH to 8.5.
[0037] (2) Fluorite roughing: Add a combined inhibitor at a dosage of 600 g / t, mix the slurry and stir for 2 min, add a collector sodium oleate at a dosage of 500 g / t, mix the slurry and stir for 2 min; the roughing flotation time is 4 min; finally, roughing concentrate and roughing tailings are obtained.
[0038] (3) The obtained rougher tailings were subjected to fluorite scavenging: scavenging I: adding the collector sodium oleate in an amount of 200 g / t, stirring for 2 min, and flotation for 3 min; scavenging II: adding the collector sodium oleate in an amount of 100 g / t, stirring for 2 min, and flotation for 3 min; the final fluorite tailings were obtained.
[0039] (4) The obtained rough concentrate is subjected to fluorite concentration: Concentration I and Concentration II: adding a combined depressant in an amount of 200 g / t, stirring for 2 min, and flotation for 3 min; Concentration III, Concentration IV and Concentration V: adding a combined depressant in an amount of 60 g / t, stirring for 2 min, and flotation for 2 min; Concentration VI and Concentration VII: adding a combined depressant in an amount of 20 g / t, stirring for 2 min, and flotation for 2 min to obtain the final fluorite concentrate.
[0040] Comparative Example 1
[0041] The process flow of this comparative example is the same as that of the embodiment. For comparison, the difference between this comparative example and embodiment 1 is that the inhibitor is single water glass. The flotation results are shown in Table 1. The specific operation steps are as follows:
[0042] The pH of the ore pulp was adjusted to 8.5. In the fluorite roughing process, water glass was selected as the inhibitor, and the dosage was 600 g / t. In the fluorite concentration: Concentration I and Concentration II: the dosage of the inhibitor water glass was 200 g / t; Concentration III, Concentration IV and Concentration V: the dosage of the inhibitor water glass was 60 g / t; Concentration VI and Concentration VII: the dosage of the inhibitor water glass was 20 g / t. The other reagent addition types, stirring time, reagent dosage and flotation time were the same as those in Example 1.
[0043] Comparative Example 2
[0044] The process flow of this comparative example is the same as that of the embodiment. As a comparison, the difference between this comparative example and embodiment 1 is that the inhibitor uses a single organic inhibitor, iminodisuccinic acid. The flotation results are shown in Table 1. The specific operation steps are as follows:
[0045] The pH of the ore pulp was adjusted to 8.5. In the fluorite roughing process, the inhibitor was selected as a single organic inhibitor, iminodisuccinic acid, with an amount of 600 g / t. In the fluorite concentration: Concentration I and Concentration II: the amount of inhibitor iminodisuccinic acid was 200 g / t; Concentration III, Concentration IV and Concentration V: the amount of inhibitor iminodisuccinic acid was 60 g / t; Concentration VI and Concentration VII: the amount of inhibitor iminodisuccinic acid was 20 g / t. The other reagent addition types, stirring time, reagent dosage and flotation time were the same as those in Example 1.
[0046] Comparative Example 3
[0047] The process flow of this comparative example is the same as that of the embodiment. For comparison, the difference between this comparative example and embodiment 1 is that the inhibitor is a single inhibitor carboxymethyl cellulose. The flotation results are shown in Table 1. The specific operation steps are as follows:
[0048] The pH of the ore pulp was adjusted to 8.5. In the fluorite roughing process, the inhibitor was selected as a single inhibitor carboxymethyl cellulose, and the dosage was 600 g / t; in the fluorite concentration: Concentration I and Concentration II: the dosage of the inhibitor carboxymethyl cellulose was 200 g / t; Concentration III, Concentration IV and Concentration V: the dosage of the inhibitor carboxymethyl cellulose was 60 g / t; Concentration VI and Concentration VII: the dosage of the inhibitor carboxymethyl cellulose was 20 g / t. The other reagent addition types, stirring time, reagent dosage and flotation time were the same as those in Example 1.
[0049] Table 1 Full process closed circuit test results of Example 1 and Comparative Examples 1 to 3
[0050]
[0051] As shown in Table 1, under the same flotation process, flotation collector, flotation pulp concentration and flotation pH conditions, compared with single flotation inorganic depressant water glass, single depressant carboxymethyl cellulose and single organic depressant iminodisuccinic acid, the combined depressor (the mass percentages of water glass, iminodisuccinic acid and carboxymethyl cellulose are 70%, 15% and 15%) can obtain higher CaF2 grade and CaF2 recovery rate, and the indicators are 95.42% and 72.81% respectively. It shows that the combined depressor of the present invention is a good flotation depressor for calcareous gangue minerals in fluorite ore flotation.
[0052] Example 2
[0053] In this embodiment, the mass percentages of water glass, iminodisuccinic acid and carboxymethyl cellulose in the components of the combined inhibitor are 65%, 25% and 10%, respectively, and the collector is a sodium oleate aqueous solution.
[0054] A high-calcium fluorite mine in Inner Mongolia has a fluorite content of 21.63% in the original ore. The main gangue minerals are calcite, quartz and mica, and the main metal minerals are pyrite and other sulfide ores. The calcite content is as high as 31.49%, and the SiO2 content is 18.36%. The flotation process also adopts a closed-circuit test process of one coarse, seven fine, and two sweeps, and the intermediate ore is returned in sequence. The flotation separation process of this embodiment is also as follows Figure 1 The flotation results are shown in Table 2. The specific steps and experimental conditions are as follows:
[0055] (1) Grind the raw ore to a grinding fineness of -0.074 mm, accounting for 75%, adjust the pulp concentration to 30%, and use pH adjuster sodium carbonate to adjust the pulp pH to 9.
[0056] (2) Fluorite roughing: Add a combined inhibitor at a dosage of 750 g / t, mix the slurry and stir for 2 min, add a collector sodium oleate at a dosage of 600 g / t, mix the slurry and stir for 2 min; the roughing flotation time is 4 min; finally, roughing concentrate and roughing tailings are obtained.
[0057] (3) The obtained rougher tailings were subjected to fluorite scavenging: Scavenging I: adding the collector sodium oleate in an amount of 300 g / t, stirring for 2 min, and flotation for 3 min; Scavenging II: adding the collector sodium oleate in an amount of 150 g / t, stirring for 2 min, and flotation for 3 min; the final fluorite tailings were obtained.
[0058] (4) The obtained rough concentrate is subjected to fluorite concentration: Concentration I and Concentration II: adding a combined depressant in an amount of 250 g / t, stirring for 2 min, and flotation for 3 min; Concentration III, Concentration IV and Concentration V: adding a combined depressant in an amount of 80 g / t, stirring for 2 min, and flotation for 2 min; Concentration VI and Concentration VII: adding a combined depressant in an amount of 25 g / t, stirring for 2 min, and flotation for 2 min to obtain the final fluorite concentrate.
[0059] Comparative Example 4
[0060] The process flow of this comparative example is the same as that of Example 2. For comparison, the difference between this comparative example and Example 2 is that the depressant is single water glass. The flotation results are shown in Table 2. The specific operation steps are as follows:
[0061] The pH of the ore pulp was adjusted to 9. In the fluorite roughing process, water glass was selected as the inhibitor, and the dosage was 750 g / t. In the fluorite concentration: Concentration I and Concentration II: the dosage of the inhibitor water glass was 250 g / t; Concentration III, Concentration IV and Concentration V: the dosage of the inhibitor water glass was 80 g / t; Concentration VI and Concentration VII: the dosage of the inhibitor water glass was 25 g / t. The other reagent addition types, stirring time, reagent dosage and flotation time were the same as those in Example 2.
[0062] Comparative Example 5
[0063] The process flow of this comparative example is the same as that of Example 2. For comparison, the difference between this comparative example and Example 2 is that the inhibitor uses water glass + iminodisuccinic acid, and the mass percentages of water glass and iminodisuccinic acid are 65% and 35%. The flotation results are shown in Table 2. The specific operation steps are as follows:
[0064] The pH of the ore pulp was adjusted to 9. In the fluorite roughing process, the inhibitor selected was organic inhibitor water glass + iminodisuccinic acid, and the dosage was 750 g / t; in fluorite concentration: Concentration I and Concentration II: the dosage of inhibitor water glass + iminodisuccinic acid was 250 g / t; Concentration III, Concentration IV and Concentration V: the dosage of inhibitor water glass + iminodisuccinic acid was 80 g / t; Concentration VI and Concentration VII: the dosage of inhibitor water glass + iminodisuccinic acid was 25 g / t. The other reagent addition types, stirring time, reagent dosage and flotation time were the same as those in Example 2.
[0065] Comparative Example 6
[0066] The process flow of this comparative example is the same as that of the embodiment. For comparison, the difference between this comparative example and embodiment 2 is that the inhibitor is water glass + carboxymethyl cellulose, the mass percentages of water glass and carboxymethyl cellulose are 65% and 35%, respectively. The flotation results are shown in Table 2. The specific operation steps are as follows:
[0067] The pH of the ore pulp was adjusted to 9. In the fluorite roughing process, the inhibitor was selected as water glass + carboxymethyl cellulose, and the dosage was 750 g / t. In the fluorite concentration: Concentration I and Concentration II: the dosage of the inhibitor water glass + carboxymethyl cellulose was 250 g / t; Concentration III, Concentration IV and Concentration V: the dosage of the inhibitor water glass + carboxymethyl cellulose was 80 g / t; Concentration VI and Concentration VII: the dosage of the inhibitor water glass + carboxymethyl cellulose was 25 g / t. The other reagent addition types, stirring time, reagent dosage and flotation time were the same as those in Example 2.
[0068] Table 2 Full process closed circuit test results of Example 2 and Comparative Examples 4 to 6
[0069]
[0070] As shown in Table 2, under the conditions of the same flotation process, flotation collector, flotation pulp concentration and flotation pH, compared with single flotation inorganic depressant water glass, water glass + iminodisuccinic acid, the combined depressor (the mass percentage of water glass, iminodisuccinic acid and carboxymethyl cellulose is 65%, 25% and 10%) can obtain higher CaF2 grade and recovery rate, and the indicators are 91.39% and 72.61% respectively. Although the recovery rate under the condition of water glass + carboxymethyl cellulose is slightly higher than that of the combined depressor, reaching 73.26%, the grade is only 88.46%. Therefore, the combined depressor described in the present invention is a good flotation depressor for calcareous gangue minerals in fluorite flotation.
Claims
1. A combined depressant for flotation separation of fluorite and calcium-containing gangue minerals, characterized in that: The combined inhibitor includes water glass, iminodisuccinic acid and carboxymethyl cellulose.
2. The combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals according to claim 1, characterized in that: The mass percentage of water glass in the combined inhibitor is 60% to 75%, the mass percentage of iminodisuccinic acid is 15% to 30%, the mass percentage of carboxymethyl cellulose is 10% to 25%, and the total mass percentage of water glass, iminodisuccinic acid and carboxymethyl cellulose is 100%.
3. Use of the combined inhibitor for flotation separation of fluorite and calcium-containing gangue minerals according to any one of claims 1 or 2 in the flotation separation of fluorite and calcareous gangue minerals.
4. The use according to claim 3, characterized in that: Fluorite concentrate and fluorite tailings are obtained from fluorite ore by flotation separation through a process of one roughing selection, seven cleaning selections and two scavenging selections.
5. The use according to claim 4, characterized in that: Combined inhibitors are added in the first roughing and seventh cleaning processes, but not in other processes.
6. The use according to claim 5, characterized in that: In the first rough selection process, the amount of combined inhibitor added is 450-750 g / t; in the seven selection processes, the amount of combined inhibitor added in selection I and selection II is 150-250 g / t, the amount of combined inhibitor added in selection III, selection IV and selection V is 50-84 g / t, and the amount of combined inhibitor added in selection VI and selection VII is 16-28 g / t.
Citation Information
Patent Citations
Wastewater defluorination application of iminodisuccinic acid (IDS) metal chelating type adsorbent
CN108996597A
Method for efficiently utilizing high calcite type low-grade scheelite and fluorite paragenic ore
CN111570081A
Flotation separation method for high-calcium fluorite mine
CN115007325A
Siliceous building material mixture
WO2010006987A1
Cited By
Collector, flotation agent and method for flotation of scheelite
CN119565785B