Method for repairing large-size defect of nickel-based superalloy guider blade

Through the combined technology of three-dimensional scanning, reverse modeling, laser selection melting and forming and vacuum brazing, the problem of large-size defect repair of nickel-based high-temperature alloy guide blades is solved, high-performance repair is achieved, reducing scrap rate and extending blades service life.

CN119216586APending Publication Date: 2024-12-31HANGFA EXCELLENT MATERIALS (ZHENJIANG) ADDITIVE MFG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411278743.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-31

AI Technical Summary

Technical Problem

The prior art is difficult to effectively repair the large-size defects of nickel-based high-temperature alloy guide blades, especially in complex internal cavity cooling channel structures. Common welding methods cannot guarantee the integrity of the repair, resulting in the scrap of the blades.

Method used

Using a combination of three-dimensional scanning, reverse modeling, laser selection melting and forming and vacuum brazing, the overall replacement of defect prefabricated parts can achieve the repair of large-sized defects, ensuring the minimization of damage and repairing the internal cavity cooling channel structure.

Benefits of technology

It significantly reduces the scrap rate of the blade, improves the repair efficiency and performance, extends the service cycle of the blade, and ensures that the size and performance of the blades after repair meet the standards.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for repairing a large-size defect of a nickel-based superalloy guider blade, which comprises the following steps: by combining three-dimensional scanning, reverse modeling, selective laser melting forming and vacuum brazing, integrally replacing a defect part by adopting a defect prefabricated part; by means of the flexibility of selective laser melting forming, prefabricated parts of various molded surfaces and structures can be prepared, defects can be removed along any curved surface of the edge of the defects, damage to the blade is reduced to the maximum extent, simultaneous repairing of an inner cavity and the outer surface can be achieved, and the rejection rate of the blade is remarkably reduced; the precision of selective laser melting forming is utilized, the size precision of a prefabricated part is high, the prefabricated part can be well matched with the blade, brazing gaps are uniform, and the performance of the repaired blade is high; by means of the high efficiency of selective laser melting forming, auxiliary products are not needed, multiple defect prefabricated parts of multiple blades can be prepared at the same time, the method is matched with the characteristic that multiple defects of the multiple blades can be repaired at the same time through vacuum brazing, and the blade repairing efficiency is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nickel-based high-temperature alloy guide vanes, and in particular relates to a method for repairing large-size defects of nickel-based high-temperature alloy guide vanes. Background Art

[0002] K477 nickel-based cast high-temperature alloy has the characteristics of high strength, good plasticity, stable structure and good casting process performance. It is used to manufacture parts such as guide vanes of gas turbines. During service, the guide vanes are subjected to thermal shock, gas corrosion and vibration loads for a long time, and are prone to large-scale defects such as cracks, large-area ablation and even falling blocks, which greatly affects the service life of the gas turbine. Limited by the expensive price of new parts and the long production cycle, blade repair has become a better choice. At present, welding is commonly used to repair guide vanes, but K477 alloy contains more Al and Ti, which is prone to intergranular liquid cracks when using fusion welding repair, resulting in repair failure. During brazing repair, the flow of liquid brazing material on the blade surface cannot be controlled, and it is only suitable for repairing small-sized defects such as cracks. In addition, in order to obtain the highest possible intake temperature, the guide vanes are usually designed with complex inner cavity cooling channel structures. When faced with these complex structures, the above two methods cannot guarantee the integrity of the inner cavity cooling channel structure and may even block the inner cavity cooling channel, ultimately causing the blades to be scrapped. For this reason, the present invention proposes a method for repairing large-size defects of nickel-based high-temperature alloy guide vanes. Summary of the invention

[0003] The object of the present invention is to provide a method for repairing large-size defects of nickel-based high-temperature alloy guide vanes to solve the problems raised in the above-mentioned background technology.

[0004] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a method for repairing large-size defects of a nickel-based high-temperature alloy guide vane, which combines three-dimensional scanning, reverse modeling, laser selective melting and vacuum brazing, uses a defective prefabricated part to replace the defective part as a whole, and achieves high-performance repair of large-size defects of the guide vane while ensuring that the damage to the blade is minimized, comprising the following steps:

[0005] Step 1: Surface treatment is performed on the guide vane after service to remove carbon deposits and coatings on the surface of the vane;

[0006] Step 2: Perform visual and fluorescent inspection on the blades to mark the type, location and size of the blade defects;

[0007] Step 3: Remove the defects of the blades by manual grinding or mechanical processing;

[0008] Step 4: Perform 3D scanning on the location marked as a large-size defect, perform reverse modeling on the acquired point cloud data, establish a blade model after removing the defect, and then compare the model with the standard model to obtain a solid model of the defect; add grinding allowance to the solid model to form a printed model, and add supports on the plane with an angle less than 55° with the horizontal plane;

[0009] Preferably, in step four, the point cloud data obtained by three-dimensional scanning is optimized and then encapsulated into a triangular mesh surface, and then the model surface is constructed and optimized, and finally the model is obtained by solid reconstruction based on the surface. The software used for three-dimensional modeling includes any one or more software such as NX and 3DMax.

[0010] Preferably, in the step 4, the solid model adds a grinding allowance of 0.05-0.1 mm on the surface to be brazed, adds a grinding allowance of 0.1-0.3 mm on the support area added to the inner cavity, does not add a grinding allowance to the unsupported area, and adds a grinding allowance of 0.2-0.4 mm on the outer surface;

[0011] Step 5: Slice the printed model after adding supports, check that the slice data is correct, set the laser selective melting parameters and print the model;

[0012] Preferably, the powder used in the step 5 laser selective melting forming is consistent with the blade composition, which is K477 powder with a particle size of 15-53μm; the laser selective melting forming parameters are: laser power 180-260W, scanning speed 850-1000mm / s, scanning spacing 0.08-0.12mm, layer thickness 0.04mm, and substrate preheating temperature 120°C.

[0013] Step 6: After printing is completed, the defective preform is cut off from the substrate, the support is removed and the surface of the preform is polished;

[0014] Step 7: Paste the brazing material foil on the surface of the blade to be brazed, assemble the processed defective prefabricated part on the blade, fix it with spot welding, add a small amount of paste brazing material to the brazing seam on the outer surface of the blade, and put it into the furnace for brazing;

[0015] Preferably, the solder foil used in step 7 contains, by mass ratio, 14.00%-17.00% Cr, 19.50%-22.50% Ni, 10.50%-13.50% W, 2.00%-3.50% B, ≤0.10% C, ≤0.05% O, ≤0.02% S, ≤0.02% P, ≤0.35% other impurity elements, and the balance is Co. The composition of the paste solder is the same as that of the foil solder; the thickness of the solder foil is 0.03-0.06 mm, and the number of pasting layers is 1-2 Layer, when pasting, press the brazing material foil on the surface to be brazed, and remove the foil at the inner cavity cooling channel; during vacuum brazing, the brazing furnace is heated to 500℃ at a rate of ≤5℃ / min, then heated to 1050℃ at a rate of ≤10℃ / min, and kept warm for 15-30min, and then heated to 1160℃ at a rate of ≤10℃ / min, and kept warm for 2h. After the end of the insulation, it is cooled to 1080℃ with the furnace and then quickly cooled to room temperature with argon gas. The process of the insulation and cooling stages is consistent with the first stage of the heat treatment of K477 material, avoiding multiple furnace entry during post-weld heat treatment;

[0016] Step 8: Use fluorescence and X-ray to inspect the repaired area to confirm that there are no defects exceeding the standard;

[0017] Step 9: Perform heat treatment on the blade to restore its performance;

[0018] Preferably, the heat treatment system in step nine is 760° C., kept at temperature for 16 hours, and rapidly cooled to room temperature by argon gas, which is consistent with the second stage process of heat treatment of K477 material;

[0019] Step 10: Grind and remove excess brazing material, and polish the outer surface of the blade;

[0020] Step 11: Perform a 3D scan on the repaired blade and compare it with the standard model to ensure that its dimensions meet the standards.

[0021] Compared with the prior art, the present invention has the following beneficial effects: the present invention makes full use of the flexibility of laser selective melting forming, and can prepare defect preforms with various profiles and structures. Therefore, when removing defects, the defects can be removed along any curved surface of the defect edge, thereby minimizing blade damage to the greatest extent, and can realize simultaneous repair of the inner cavity cooling channel and the outer surface profile, thereby significantly reducing the scrap rate of the blade;

[0022] The present invention makes full use of the accuracy of laser selective melting forming, and can prepare defect preforms with high dimensional accuracy, which can form a good match with the base of the blade after the defects are removed, ensuring the uniformity of the brazing gap. The repaired blade has higher performance and can effectively extend the service life of the blade.

[0023] The present invention makes full use of the high efficiency of laser selective melting forming, does not require auxiliary products such as molds, shells, cores, etc., and can simultaneously prepare multiple defect preforms of multiple blades. It is compatible with the characteristic of vacuum brazing that can simultaneously repair multiple defects of multiple blades, and can greatly improve the repair efficiency of blades. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] This embodiment provides a technical solution: a method for repairing large-size defects of a nickel-based high-temperature alloy guide vane, which replaces the defective part as a whole by combining three-dimensional scanning, reverse modeling, laser selective melting and vacuum brazing, and achieves high-performance repair of large-size defects of the guide vane while minimizing damage to the blade, including the following steps:

[0027] Step 1: Surface treatment is performed on the guide vane after service to remove carbon deposits and coatings on the surface of the vane;

[0028] Step 2: Perform visual and fluorescent inspection on the blades to mark the type, location and size of the blade defects;

[0029] Step 3: Remove the defects of the blades by manual grinding or mechanical processing;

[0030] Step 4: Perform 3D scanning on the location marked as a large-size defect, perform reverse modeling on the acquired point cloud data, establish a blade model after removing the defect, and then compare the model with the standard model to obtain a solid model of the defect; add grinding allowance to the solid model to form a printed model, and add supports on the plane with an angle less than 55° with the horizontal plane;

[0031] Step 5: Slice the printed model after adding supports, check that the slice data is correct, set the laser selective melting parameters and print the model;

[0032] Step 6: After printing is completed, the defective preform is cut off from the substrate, the support is removed and the surface of the preform is polished;

[0033] Step 7: Paste the brazing material foil on the surface of the blade to be brazed, assemble the processed defective prefabricated part on the blade, fix it with spot welding, add a small amount of paste brazing material to the brazing seam on the outer surface of the blade, and put it into the furnace for brazing;

[0034] Step 8: Use fluorescence and X-ray to inspect the repaired area to confirm that there are no defects exceeding the standard;

[0035] Step 9: Perform heat treatment on the blade to restore its performance;

[0036] Step 10: Grind and remove excess brazing material, and polish the outer surface of the blade;

[0037] Step 11: Perform a 3D scan on the repaired blade and compare it with the standard model to ensure that its dimensions meet the standards.

[0038] In this embodiment, preferably, in step four, the solid model adds a grinding allowance of 0.05 mm on the surface to be brazed, adds a grinding allowance of 0.1 mm on the support area on the inner cavity, does not add a grinding allowance to the unsupported area, and adds a grinding allowance of 0.2 mm on the outer surface.

[0039] In this embodiment, preferably, the powder used in step five laser selective melting is consistent with the composition of the blade, which is K477 powder with a particle size of 15-53μm; laser selective melting parameters are: laser power 180-260W, scanning speed 850mm / s, scanning spacing 0.08mm, layer thickness 0.04mm, and substrate preheating temperature 120℃.

[0040] In this embodiment, preferably, the solder foil used in step seven has a composition calculated by mass ratio, including 14.00% Cr, 19.50% Ni, 10.50% W, 2.00% B, ≤0.10% C, ≤0.05% O, ≤0.02% S, ≤0.02% P, ≤0.35% other impurity elements, and the balance is Co. The composition of the paste solder is the same as that of the foil solder; the thickness of the solder foil is 0.06 mm, the number of pasting layers is 1, and the solder foil is pressed tightly during pasting. On the surface to be brazed, remove the foil strip at the inner cavity cooling channel; during vacuum brazing, the brazing furnace is heated to 500℃ at a rate of 5℃ / min, then heated to 1050℃ at a rate of 10℃ / min, kept warm for 15 minutes, and then heated to 1160℃ at a rate of 10℃ / min, kept warm for 2 hours. After the insulation, the furnace is cooled to 1080℃ and then quickly cooled to room temperature with argon gas. The process of the insulation and cooling stages is consistent with the first stage of heat treatment of K477 material to avoid multiple entries into the furnace during post-weld heat treatment.

[0041] In this embodiment, preferably, the heat treatment system of step nine is 760° C., kept warm for 16 hours, and quickly cooled to room temperature with argon gas, which is consistent with the second stage process of heat treatment of K477 material.

[0042] In this embodiment, preferably, in step four, the point cloud data obtained by the three-dimensional scanning is optimized and then encapsulated into a triangular mesh surface, and then the model surface is constructed and optimized, and finally the model is obtained by solid reconstruction based on the surface. The software used for three-dimensional modeling includes any one or more software such as NX and 3DMax.

[0043] Example 2

[0044] A method for repairing large-size defects of a nickel-based high-temperature alloy guide vane is provided. The defective part is replaced as a whole by combining three-dimensional scanning, reverse modeling, laser selective melting and vacuum brazing. Under the premise of minimizing the damage to the blade, high-performance repair of large-size defects of the guide vane is achieved. The method comprises the following steps:

[0045] Step 1: Surface treatment is performed on the guide vane after service to remove carbon deposits and coatings on the surface of the vane;

[0046] Step 2: Perform visual and fluorescent inspection on the blades to mark the type, location and size of the blade defects;

[0047] Step 3: Remove the defects of the blades by manual grinding or mechanical processing;

[0048] Step 4: Perform 3D scanning on the location marked as a large-size defect, perform reverse modeling on the acquired point cloud data, establish a blade model after removing the defect, and then compare the model with the standard model to obtain a solid model of the defect; add grinding allowance to the solid model to form a printed model, and add supports on the plane with an angle less than 55° with the horizontal plane;

[0049] Step 5: Slice the printed model after adding supports, check that the slice data is correct, set the laser selective melting parameters and print the model;

[0050] Step 6: After printing is completed, the defective preform is cut off from the substrate, the support is removed and the surface of the preform is polished;

[0051] Step 7: Paste the brazing material foil on the surface of the blade to be brazed, assemble the processed defective prefabricated part on the blade, fix it with spot welding, add a small amount of paste brazing material to the brazing seam on the outer surface of the blade, and put it into the furnace for brazing;

[0052] Step 8: Use fluorescence and X-ray to inspect the repaired area to confirm that there are no defects exceeding the standard;

[0053] Step 9: Perform heat treatment on the blade to restore its performance;

[0054] Step 10: Grind and remove excess brazing material, and polish the outer surface of the blade;

[0055] Step 11: Perform a 3D scan on the repaired blade and compare it with the standard model to ensure that its dimensions meet the standards.

[0056] In this embodiment, preferably, in step four, the solid model adds a grinding allowance of 0.1 mm on the surface to be brazed, adds a grinding allowance of 0.3 mm on the support area on the inner cavity, does not add a grinding allowance to the unsupported area, and adds a grinding allowance of 0.4 mm on the outer surface.

[0057] In this embodiment, preferably, the powder used in step five laser selective melting forming is consistent with the composition of the blade, which is K477 powder with a particle size of 15-53μm; laser selective melting forming parameters: laser power 260W, scanning speed 1000mm / s, scanning spacing 0.12mm, layer thickness 0.04mm, substrate preheating temperature 120℃.

[0058] In this embodiment, preferably, the solder foil used in step seven contains 17.00% Cr, 22.50% Ni, 13.50% W, 3.50% B, ≤0.10% C, ≤0.05% O, ≤0.02% S, ≤0.02% P, ≤0.35% other impurity elements, and the balance is Co. The composition of the paste solder is the same as that of the foil solder; the thickness of the solder foil is 0.05 mm, the number of pasting layers is 2, and the solder foil is pasted Press it tightly on the surface to be brazed, and remove the foil in the cooling channel; during vacuum brazing, the brazing furnace is heated to 500℃ at a rate of 3℃ / min, then heated to 1050℃ at a rate of 8℃ / min, kept warm for 30min, and then heated to 1160℃ at a rate of 10℃ / min, kept warm for 2h. After the insulation, it is cooled to 1080℃ with the furnace and then quickly cooled to room temperature with argon gas. The process of the insulation and cooling stages is consistent with the first stage of heat treatment of K477 material to avoid multiple entries into the furnace during post-weld heat treatment.

[0059] In this embodiment, preferably, the heat treatment system of step nine is 760° C., kept warm for 16 hours, and quickly cooled to room temperature with argon gas, which is consistent with the second stage process of heat treatment of K477 material.

[0060] In this embodiment, preferably, in step four, the point cloud data obtained by the three-dimensional scanning is optimized and then encapsulated into a triangular mesh surface, and then the model surface is constructed and optimized, and finally the model is obtained by solid reconstruction based on the surface. The software used for three-dimensional modeling includes any one or more software such as NX and 3DMax.

[0061] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for repairing large-size defects of nickel-based high-temperature alloy guide vanes, characterized in that: By combining 3D scanning, reverse modeling, laser selective melting and vacuum brazing, the defective part is replaced as a whole, and high-performance repair of large-size defects in the guide vane is achieved while minimizing the damage to the blade. The process includes the following steps: Step 1: Surface treatment is performed on the guide vane after service to remove carbon deposits and coatings on the surface of the vane; Step 2: Perform visual and fluorescent inspection on the blades to mark the type, location and size of the blade defects; Step 3: Remove the defects of the blades by manual grinding or mechanical processing; Step 4: Perform 3D scanning on the location marked as a large-size defect, perform reverse modeling on the acquired point cloud data, establish a blade model after removing the defect, and then compare the model with the standard model to obtain a solid model of the defect; add grinding allowance to the solid model to form a printed model, and add supports on the plane with an angle less than 55° with the horizontal plane; Step 5: Slice the printed model after adding supports, check that the slice data is correct, set the laser selective melting parameters and print the model; Step 6: After printing is completed, the defective preform is cut off from the substrate, the support is removed and the surface of the preform is polished; Step 7: Paste the brazing material foil on the surface of the blade to be brazed, assemble the processed defective prefabricated part on the blade, fix it with spot welding, add a small amount of paste brazing material at the brazing seam on the outer surface of the blade, and put it into the furnace for brazing; Step 8: Use fluorescence and X-ray to inspect the repaired area to confirm that there are no defects exceeding the standard; Step 9: Perform heat treatment on the blade to restore its performance; Step 10: Grind and remove excess brazing material, and polish the outer surface of the blade; Step 11: Perform a 3D scan on the repaired blade and compare it with the standard model to ensure that its dimensions meet the standards.

2. The method for repairing large-size defects of a nickel-based high-temperature alloy guide vane according to claim 1, characterized in that: In the step 4, the point cloud data obtained by the 3D scanning is optimized and then encapsulated into a triangular mesh surface, and then the model surface is constructed and optimized. Finally, the solid reconstruction is performed based on the surface to obtain the model. The software used for 3D modeling includes any one or more software such as NX and 3DMax.

3. The method for repairing large-size defects of a nickel-based high-temperature alloy guide vane according to claim 1, characterized in that: In the step 4, the solid model adds a grinding allowance of 0.05-0.1 mm on the surface to be brazed, adds a grinding allowance of 0.1-0.3 mm on the support area of ​​the inner cavity, does not add a grinding allowance to the unsupported area, and adds a grinding allowance of 0.2-0.4 mm on the outer surface.

4. The method for repairing large-size defects of a nickel-based high-temperature alloy guide vane according to claim 1, characterized in that: The powder used in the step five laser selective melting forming is consistent with the composition of the blade. For the blade with a matrix composition of K477, the powder composition used is also K477, and the particle size is 15-53μm; laser selective melting forming parameters: laser power 180-260W, scanning speed 850-1000mm / s, scanning spacing 0.08-0.12mm, layer thickness 0.04mm, substrate preheating temperature 120℃.

5. The method for repairing large-size defects of a nickel-based high-temperature alloy guide vane according to claim 1, characterized in that: The solder foil used in step 7 contains, by mass ratio, 14.00%-17.00% Cr, 19.50%-22.50% Ni, 10.50%-13.50% W, 2.00%-3.50% B, ≤0.10% C, ≤0.05% O, ≤0.02% S, ≤0.02% P, ≤0.35% other impurity elements, and the balance is Co. The composition of the paste solder is the same as that of the foil solder; the thickness of the solder foil is 0.03-0.06mm, and the number of pasted layers is 1-2 layers. When pasting, press the brazing material foil tightly against the surface to be brazed, and remove the foil at the inner cavity cooling channel; during vacuum brazing, the brazing furnace is heated to 500℃ at a rate of ≤5℃ / min, then heated to 1050℃ at a rate of ≤10℃ / min, kept warm for 15-30min, and then heated to 1160℃ at a rate of ≤10℃ / min, kept warm for 2h. After the insulation, it is cooled to 1080℃ with the furnace and then quickly cooled to room temperature with argon gas. The process of the insulation and cooling stages is consistent with the first stage of the heat treatment of K477 material to avoid multiple entries into the furnace during post-weld heat treatment.

6. The method for repairing large-size defects of a nickel-based high-temperature alloy guide vane according to claim 1, characterized in that: The heat treatment system of step nine is 760° C., keeping warm for 16 hours, and rapidly cooling to room temperature with argon gas, which is consistent with the second stage process of heat treatment of K477 material.