Double-layer coating as well as preparation method and application thereof
By using double-layer coatings and using the combination of ceramic precursors and resins, the scale, corrosion and high energy consumption problems caused by the use of enamel or stainless steel materials in the water heater are solved, and the effects of low adhesion, corrosion and energy efficiency improvement are achieved.
Patent Information
- Application Number
- CN202311682247.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2025-06-10
AI Technical Summary
The long-term use of enamel or stainless steel materials in the home appliance industry has problems of scale, corrosion and high energy consumption.
A double-layer coating is used, including base coating and top coating. The base coating is composed of ceramic precursor and resin. The ceramic precursor is composed of polysilane compounds and metal precursors. Through chemical grafting and structuring of micro-nano structures, low adhesion performance and excellent corrosion resistance are achieved.
Effectively prevent scale generation, improve corrosion resistance, reduce energy consumption, and eliminate the need for heavy metals. It is suitable for surface treatment of heaters such as water heaters.
Smart Images

Figure HDA0004596572740000011 
Figure HDA0004596572740000012
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a double-layer coating, a preparation method thereof, and an application thereof. Background Art
[0002] Coatings are a type of liquid or solid material that is coated on the surface of an object and can form a film under certain conditions to perform functions such as protection, decoration, or other special functions (insulation, rust prevention, mildew prevention, heat resistance, etc.). Coatings can be classified into architectural coatings, automotive coatings, household appliance coatings, wood coatings, and so on according to their uses. Among them, with the development of the household appliance industry, the requirements for the performance and functionality of household appliance coatings are increasing day by day.
[0003] In water heater products, enamel and stainless steel are the most widely used coating materials. Among them, enamel is widely used in water heater production due to its high hardness, excellent scratch resistance and high temperature resistance, and stainless steel has also won a large number of applications due to its excellent corrosion resistance.
[0004] However, enamel has the following disadvantages: ① high sintering temperature (most are greater than 800 °C), high energy consumption; ② there is a risk of heavy metals; ③ low yield, and defects such as porcelain explosion and enamel burning are likely to occur; ④ roughing pretreatment such as sandblasting is required; ⑤ the surface is difficult to clean, and problems such as scale are likely to occur during the operation of the heater.
[0005] Stainless steel has poor heat resistance, starts to oxidize at about 250 °C, and its corrosion resistance decreases; and the surface is difficult to clean, and problems such as scale are likely to occur during the operation of the heater. Summary of the Invention
[0006] The present invention aims to solve at least one of the technical problems existing in the related art. For this reason, the present invention provides a double-layer coating, a preparation method thereof, and an application thereof. The double-layer coating formed by the double-layer coating has excellent properties such as low viscosity, high adhesion, and corrosion resistance, aiming to solve the technical problems such as scale, corrosion, and high energy consumption existing in the long-term use of enamel or stainless steel materials in the water heaters of the household appliance industry.
[0007] In a first aspect, the present invention provides a double-layer coating, including a bottom layer coating and a top layer coating. The bottom layer coating includes a ceramic precursor and a resin. The ceramic precursor is composed of a polysilane compound and a metal precursor. The polysilane compound is selected from one or more of polycarbosilane, polyborosilazane, and polysilicon boron carbonitride. The metal precursor is selected from one or more of a zirconium precursor, an aluminum precursor, and a titanium precursor.
[0008] According to the double-layer coating provided by the present invention, the mass ratio of the polysilane compound to the metal precursor is 3:1 - 1:6.
[0009] According to the double-layer coating provided by the present invention, the resin is a polysiloxane resin and / or an epoxy resin, preferably a mixture of a polysiloxane resin and an epoxy resin with a mass ratio of 20:0 - 8:15.
[0010] According to the double-layer coating provided by the present invention, the mass ratio of the ceramic precursor to the resin is 99:1 - 10:90.
[0011] According to the double-layer coating provided by the present invention, the bottom coating further comprises one or more of a filler, a solvent, and an additive.
[0012] Preferably, the filler is selected from one or more of silicon carbide, talcum powder, glass flakes, basalt flakes, muscovite, zinc phosphate, aluminum phosphate, low-melting glass powder, silica, and inorganic pigments, and the mass of the filler accounts for 0.1 - 50% of the mass of the bottom coating;
[0013] The solvent is selected from one or more of alkane solvents, ether solvents, ketone solvents, benzene derivative solvents, and ester solvents, and the mass of the solvent accounts for 0.1 - 50% of the mass of the bottom coating;
[0014] The additive is selected from one or more of a dispersant, an anti-corrosion agent, and a wetting and leveling agent, and the mass of the additive accounts for 0.1 - 5% of the mass of the bottom coating.
[0015] According to the double-layer coating provided by the present invention, the surface coating is composed by mass percentage: 10% - 50% of silica sol, 1 - 25% of epoxy-modified polysiloxane, 0 - 20% of polysilane compounds, 0.1 - 5% of anti-graffiti additives, and 10 - 70% of a solvent;
[0016] The solvent is preferably butyl acetate.
[0017] In a second aspect, the present invention provides a preparation method of the above double-layer coating, which includes two parts: the preparation of the bottom coating and the preparation of the surface coating.
[0018] Among them, the preparation method of the bottom coating includes:
[0019] Mix a polysilane compound and a metal precursor to obtain a ceramic precursor, namely component A;
[0020] Mix and grind the raw materials other than the ceramic precursor to obtain component B, with a fineness ≤ 15 μm;
[0021] Finally, mix component A and component B to obtain the bottom coating.
[0022] The preparation method of the surface coating includes:
[0023] Mix silica sol, epoxy-modified siloxane, polysilane compounds, anti-graffiti aids and a solvent to obtain the topcoat. Stirring mixing is preferably used, and the stirring rate is 100 - 2000 r / min.
[0024] In a third aspect, the present invention provides a double-layer coating formed from the above double-layer coating.
[0025] In a fourth aspect, the present invention provides an article with a coating, which article contains a substrate and a coating attached to at least a part of the surface of the substrate, and the coating is a double-layer coating formed from the above double-layer coating.
[0026] For the article with a coating provided by the present invention, the substrate is a metal substrate, a glass substrate, a ceramic substrate, an enamel substrate, a polymer substrate, or a composite substrate of two or more of the above substrates.
[0027] For the article with a coating provided by the present invention, the article is a household appliance, preferably a water heater.
[0028] One or more of the above technical solutions in the embodiments of the present invention have at least one of the following technical effects:
[0029] The present invention provides a double-layer coating, its preparation method and application. The bottom coating uses the copolymerization product obtained by the reaction of a ceramic precursor and a resin as the main resin, and the ceramic precursor is composed of a specific polysilane compound and a metal precursor, realizing the performance of low adhesion on the material surface, thereby effectively preventing the formation of water scale, improving the anti-corrosion performance and reducing energy consumption at the same time.
[0030] Furthermore, the topcoat of the present invention also has excellent low surface energy, can further prevent the formation of water scale, and is particularly suitable for electrical appliances such as water heaters that heat water.
[0031] The additional aspects and advantages of the present invention will be partly given in the following description, partly will become obvious from the following description, or will be understood through the practice of the present invention. Description of the Drawings
[0032] Figure 1 The state of water scale on the heater coated with the coating of Example 1 of the present invention;
[0033] Figure 2 The state of water scale of the blank control. Detailed Description of the Embodiments
[0034] The following further describes in detail the embodiments of the present invention in conjunction with the embodiments. The following embodiments are used to illustrate the present invention, but cannot be used to limit the scope of the present invention.
[0035] In the description of this specification, the descriptions referring to terms such as "one embodiment", "some embodiments", "example", "specific example", or "some examples" mean that the specific features, structures, materials, or characteristics described in connection with the embodiment or example are included in at least one embodiment or example of the embodiments of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in a suitable manner in any one or more embodiments or examples. In addition, without contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples.
[0036] In a first aspect, the present invention provides a double-layer coating, including a bottom layer coating and a top layer coating. The bottom layer coating includes a ceramic precursor and a resin. The ceramic precursor is composed of a polysilane compound and a metal precursor. The polysilane compound is selected from one or more of polycarbosilane, polyborosilazane, and polysilboron carbonitride. The metal precursor is selected from one or more of a zirconium precursor, an aluminum precursor, and a titanium precursor.
[0037] The present invention uses the copolymerization product obtained by the reaction of a ceramic precursor with excellent reactivity and a resin as the main resin of the bottom layer coating. The ceramic precursor is composed of specific polysilane compounds and metal precursors. By means of chemically grafting low-surface-energy groups and constructing micro-nano structures, the performance of low adhesion on the material surface is achieved, thereby effectively preventing the formation of water scale. At the same time, the present invention uses the copolymerization product obtained by the reaction of a ceramic precursor and a resin as the main resin of the bottom layer coating, and the formed film has excellent denseness, improving the anti-corrosion performance. In addition, this coating system has excellent adhesion performance. Therefore, without roughening such as sandblasting, only removing the oil stain on the surface of the workpiece can achieve excellent adhesion between the coating and the blank substrate. Compared with enamel materials, the bottom layer coating of the present invention can achieve excellent adhesion between the coating and the substrate without using heavy metals such as cobalt and nickel. Moreover, since the present invention uses an organic polymer material as the main resin, excellent adhesion performance can be achieved at low temperatures (below 300 °C). Compared with the sintering temperature of enamel greater than 850 °C, the energy consumption is significantly reduced. Generally speaking, the coating of the present invention is significantly superior to the existing enamel and stainless steel coating materials, and is particularly suitable for the surface treatment of water heater heaters.
[0038] In the present invention, the zirconium precursor refers to a class of organic polymers with a main chain of Zr-O and reactive groups on the side chain, which can be converted into inorganic substances under conditions such as heating.
[0039] The aluminum precursor refers to a class of organic polymers with a main chain of Al-O and reactive groups on the side chain, which can be converted into inorganic substances under conditions such as heating.
[0040] The titanium precursor refers to a class of organic polymers with a main chain of Ti-O and reactive groups on the side chains, which can be converted into inorganic substances under conditions such as heating.
[0041] In some embodiments of the present invention, the mass ratio of the polysilane compound to the metal precursor is 3:1 - 1:6.
[0042] The resin described in the present invention is a common coating resin, which can react stably with the ceramic precursor. In some embodiments of the present invention, the resin is polysiloxane and / or epoxy resin. More preferably, the resin is a mixture of polysiloxane resin and epoxy resin with a mass ratio of 20:0 - 8:15.
[0043] In some embodiments of the present invention, the mass ratio of the ceramic precursor to the resin is 99:1 - 10:90.
[0044] In some embodiments of the present invention, the bottom coating further includes one or more of a filler, a solvent, and an additive.
[0045] The addition of the filler can, on the one hand, give the coating a certain color, and on the other hand, make the coating denser and more conducive to corrosion prevention. In some embodiments of the present invention, the filler is selected from one or more of silicon carbide, talcum powder, glass flakes, basalt flakes, muscovite, zinc phosphate, aluminum phosphate, low-melting glass powder, white carbon black, and inorganic pigments. The mass of the filler accounts for 0.1 - 50% of the mass of the bottom coating, preferably 30 - 50%.
[0046] In some embodiments of the present invention, the solvent is selected from one or more of alkane solvents, ether solvents, ketone solvents, benzene derivative solvents, and ester solvents. The mass of the solvent accounts for 0.1 - 50% of the mass of the bottom coating, preferably 20 - 40%.
[0047] Among them, the alkane solvents are selected from one or more of n-hexane, n-octane, n-decane, chloroform, dichloromethane, dichloroethylene, and mineral oil.
[0048] The ether solvents are selected from at least one of diethyl ether, petroleum ether, and dibutyl ether.
[0049] The ketone solvents are selected from at least one of acetone, methyl ethyl ketone, cyclohexanone, and isophorone.
[0050] The benzene derivative solvents are selected from at least one of toluene, m-xylene, p-xylene, o-xylene, and chlorobenzene.
[0051] The ester solvents are selected from ethyl acetate and propyl propionate, preferably ethyl acetate.
[0052] In some embodiments of the present invention, the auxiliary agent is selected from one or more of auxiliary agents such as dispersants, corrosion inhibitors, wetting and leveling agents, and anti-graffiti auxiliary agents that can enhance the performance of the coating composition, and the mass of the auxiliary agent accounts for 0.1-5% of the mass of the primer coating.
[0053] In some embodiments of the present invention, the topcoat is composed by mass percentage: 10% to 50% of silica sol, 1-25% of epoxy-modified siloxane, 0 to 20% of polysilane compounds, 0.1 to 5% of anti-graffiti auxiliary agent, and 10 to 70% of solvent.
[0054] In the topcoat, the solvent is preferably butyl acetate. Butyl acetate can dissolve and mix each component well.
[0055] Second, the present invention provides a preparation method of the above double-layer coating, including two parts: primer coating preparation and topcoat preparation.
[0056] Among them, the preparation method of the primer coating includes:
[0057] Mix the polysilane compound and the metal precursor to obtain a ceramic precursor, that is, component A;
[0058] Mix and grind the raw materials other than the ceramic precursor to obtain component B, and the fineness is ≤15μm;
[0059] Finally, mix component A and component B to obtain the primer coating.
[0060] The preparation method of the topcoat includes:
[0061] Mix silica sol, epoxy-modified siloxane, polysilane compounds, anti-graffiti auxiliary agent and solvent to obtain the topcoat.
[0062] Among them, during the preparation of the primer coating and the topcoat, mixing can be carried out by conventional means in the art such as stirring and mixing, and the stirring speed is preferably 100-2000 r / min.
[0063] When grinding component B, common equipment in the art such as sand mills, basket grinders, high-speed dispersers, etc. can be used to grind the mixed material to a fineness of ≤15μm.
[0064] In some embodiments of the present invention, when obtaining component B by mixing, the resin is first dispersed in the solvent, and then the remaining materials are added and mixed evenly.
[0065] It can be understood that the component addition order, stirring speed, stirring time, grinding method, etc. mentioned in the preparation method are only typical values in the experimental process. If the order and processing parameters are adjusted to others, coatings with similar properties can also be obtained, and most are only differences in production efficiency.
[0066] In a third aspect, the present invention provides a double-layer coating formed from the above double-layer coating material.
[0067] Specifically, during the formation of the coating, the bottom coating material is first applied to the surface of the substrate by common construction methods such as spraying, brushing, or roll coating. After drying, a bottom coating is formed. Then, the top coating material is applied to the dried bottom coating, and finally a double-layer coating is formed.
[0068] In some embodiments of the present invention, for better long-term effectiveness and scale inhibition, the thickness of the bottom coating is 15 - 25 μm and the thickness of the top coating is 4 - 7 μm.
[0069] In a fourth aspect, the present invention provides an article with a coating. The article includes a substrate and a coating attached to at least a part of the surface of the substrate, and the coating is a coating formed from the above coating composition.
[0070] In some embodiments of the present invention, the substrate is a metal substrate, a glass substrate, a ceramic substrate, an enamel substrate, a polymer substrate, or a composite substrate of two or more of the above substrates.
[0071] In some embodiments of the present invention, the article is a household appliance, preferably a water heater.
[0072] There are many household appliances, such as microwave ovens, ovens, range hoods, cooktops, vacuum cleaners, dishwashers, air conditioners, refrigerators, washing machines, water heaters, etc. They all need to be coated with a coating, but the coating of the present invention is more suitable for water heaters because this double-layer coating material specifically solves problems such as easy scale formation and corrosion, and can also withstand a certain high temperature (about 100 °C), which is different from the coating developed by the applicant before that is more suitable for household appliances with higher temperature resistance requirements (about 400 °C) such as microwave ovens and ovens.
[0073] Specific embodiments will be described below.
[0074] In the following embodiments, where specific technologies or conditions are not indicated, they are carried out according to the technologies or conditions described in the literature in the field or according to the product instructions. For reagents or instruments whose manufacturers are not indicated, they are all conventional products that can be obtained through regular channels.
[0075] In the following embodiments, the zirconium precursor used is an organic polymer with a main chain of Zr - O and side chains containing hydrogen, vinyl, and methyl groups. The aluminum precursor used is an organic polymer with a main chain of Al - O and side chains containing hydrogen, vinyl, and methyl groups. The titanium precursor used is an organic polymer with a main chain of Ti - O and side chains containing hydrogen, vinyl, and methyl groups.
[0076] Example 1
[0077] This embodiment provides a double-layer coating, including a bottom-layer coating and a top-layer coating.
[0078] Among them, the composition of the bottom-layer coating by mass percentage is as follows: polycarbosilane 4%, zirconium precursor 11%, polysiloxane resin 20%, talcum powder 5%, glass flake 15%, white carbon black 2%, low-melting glass powder 3%, copper chromite black 13%, diethylene glycol butyl ether 10.4%, propylene glycol methyl ether acetate 16%, dispersant 0.5%, wetting and leveling agent 0.1%. Its preparation method is as follows:
[0079] (1) Preparation of component A:
[0080] Weigh 4% polycarbosilane and 11% zirconium precursor, and mix them evenly.
[0081] (2) Preparation of component B:
[0082] Stir 20% polysiloxane resin with 10.4% diethylene glycol butyl ether and 16% propylene glycol methyl ether acetate at 500 r / min until evenly dissolved, and then add 0.5% dispersant, 0.1% wetting and leveling agent, 5% talcum powder, 15% glass flake, 2% white carbon black, 3% low-melting glass powder, and 13% copper chromite black one by one, and pre-stir at 1000 r / min until the materials are evenly mixed.
[0083] Use a sand mill to grind the above premix at 2000 r / min until the fineness ≤ 15 μm.
[0084] (3) Preparation of the bottom-layer coating:
[0085] Mix the above component A and component B, and stir at 600 r / min until evenly mixed to obtain the bottom-layer coating.
[0086] Among them, the composition of the top-layer coating by mass percentage is as follows: silica sol 10%, epoxy-modified siloxane 25%, polysilazane 20%, anti-graffiti additive 3%, butyl acetate 42%. Its preparation method is as follows:
[0087] Add 10% silica sol, 25% epoxy-modified siloxane, 20% polysilazane, 3% anti-graffiti additive, and 42% butyl acetate into the stirring tank one by one, and stir at 1000 r / min until evenly mixed to obtain the top-layer coating.
[0088] Example 2
[0089] This embodiment provides a double-layer coating, including a bottom-layer coating and a top-layer coating.
[0090] Among them, the composition of the bottom coating by mass percentage is: polysilicon boron carbonitride 2%, aluminum precursor 11.4%, polysiloxane resin 8%, epoxy resin 15%, silicon carbide 3%, glass flake 10%, mica 5%, zinc phosphate 3%, low-melting glass powder 3%, copper chromite black 17%, petroleum ether 5%, butyl acetate 5%, propylene glycol methyl ether acetate 12%, dispersant 0.5%, wetting and leveling agent 0.1%. The preparation method is as follows:
[0091] (1) Preparation of component A:
[0092] Weigh 2% polysilicon boron carbonitride and 11.4% aluminum precursor, and mix them evenly.
[0093] (2) Preparation of component B:
[0094] Add 8% polysiloxane resin, 15% epoxy resin, 5% petroleum ether, 5% butyl acetate, and 12% propylene glycol methyl ether acetate into a stirrer and stir at 500 r / min until evenly dissolved. Then add 0.5% dispersant, 0.1% wetting and leveling agent, 3% silicon carbide, 10% glass flake, 5% mica, 3% zinc phosphate, 3% low-melting glass powder, and 17% copper chromite black one by one, and pre-stir at 900 r / min until the materials are evenly mixed.
[0095] Use a sand mill to grind the above premix at 2000 r / min until the fineness is ≤ 15 μm.
[0096] (3) Preparation of the bottom coating:
[0097] Mix the above component A and component B, and stir at 400 r / min until evenly mixed to prepare the bottom coating.
[0098] Among them, the composition of the top coating by mass percentage is: silica sol 50%, epoxy-modified siloxane 1%, polysilazane 13%, anti-graffiti additive 2%, butyl acetate 34%. The preparation method is as follows:
[0099] Add 50% silica sol, 1% epoxy-modified siloxane, 13% polysilazane, 2% anti-graffiti additive, and 34% butyl acetate into a stirring tank one by one, and stir at 100 r / min until evenly mixed to prepare the top coating.
[0100] Example 3
[0101] This example provides a double-layer coating, including a bottom coating and a top coating.
[0102] Among them, the bottom coating is composed by mass percentage as follows: polyborosilazane 4%, titanium precursor 12%, polysiloxane resin 12%, epoxy resin 17%, silicon carbide 3%, talcum powder 3%, basalt flakes 7%, zinc phosphate 4%, aluminum phosphate 4%, low-melting glass powder 5%, copper chromite black 10%, p-xylene 6%, propylene glycol methyl ether acetate 12.4%, dispersant 0.5%, wetting and leveling agent 0.1%. Its preparation method is as follows:
[0103] (1) Preparation of component A:
[0104] Weigh 4% polyborosilazane and 12% titanium precursor, and mix them evenly.
[0105] (2) Preparation of component B:
[0106] Add 12% polysiloxane resin, 17% epoxy resin, 6% p-xylene, and 12.4% propylene glycol methyl ether acetate into a stirrer, stir at 700 r / min until evenly dissolved, and then add 0.5% dispersant, 0.1% wetting and leveling agent, 3% silicon carbide, 3% talcum powder, 7% basalt flakes, 4% zinc phosphate, 4% aluminum phosphate, 5% low-melting glass powder, and 10% copper chromite black one by one, and pre-stir at 1000 r / min until the materials are evenly mixed.
[0107] Use a sand mill to grind the above premix at 2000 r / min until the fineness is ≤15 μm.
[0108] (3) Preparation of the bottom coating:
[0109] Mix the above component A and component B, and stir at 600 r / min until evenly mixed to obtain the bottom coating.
[0110] Among them, the top coating is composed by mass percentage as follows: silica sol 30%, epoxy-modified siloxane 15%, polysilazane 12%, anti-graffiti additive 5%, butyl acetate 38%. Its preparation method is as follows:
[0111] Add 30% silica sol, 15% epoxy-modified siloxane, 12% polysilazane, 5% anti-graffiti additive, and 38% butyl acetate into a stirring tank one by one, and stir at 700 r / min until evenly mixed to obtain the top coating.
[0112] Example 4
[0113] This example provides a double-layer coating, including a bottom coating and a top coating.
[0114] Among them, the bottom coating is composed by mass percentage as follows: 15% polyborosilazane, 5% zirconium precursor, 10% polysiloxane resin, 10% epoxy resin, 10% silicon carbide, 4% basalt flakes, 4% zinc phosphate, 5% low-melting glass powder, 10% copper chromeblack, 10% p-xylene, 16.4% propylene glycol methyl ether acetate, 0.5% dispersant, and 0.1% wetting and leveling agent. Its preparation method is as follows:
[0115] (1) Preparation of component A:
[0116] Weigh 15% polyborosilazane and 5% zirconium precursor, and mix them evenly.
[0117] (2) Preparation of component B:
[0118] Stir 10% polysiloxane resin, 10% epoxy resin, 10% p-xylene, and 16.4% propylene glycol methyl ether acetate at 800 r / min until they are evenly dissolved. Then add 0.5% dispersant, 0.1% wetting and leveling agent, 10% silicon carbide, 4% basalt flakes, 4% zinc phosphate, 5% low-melting glass powder, and 10% copper chromeblack one by one, and pre-stir at 1000 r / min until the materials are evenly mixed.
[0119] Use a sand mill to grind the above premix at 2000 r / min until the fineness is ≤ 15 μm.
[0120] (3) Preparation of the bottom coating:
[0121] Mix the above component A and component B, and stir at 700 r / min until they are evenly mixed to prepare the bottom coating.
[0122] Among them, the top coating is composed by mass percentage as follows: 20% silica sol, 20% epoxy-modified siloxane, 20% polysilazane, 0.5% anti-graffiti additive, and 39.5% butyl acetate. Its preparation method is as follows:
[0123] Add 20% silica sol, 20% epoxy-modified siloxane, 20% polysilazane, 0.5% anti-graffiti additive, and 39.5% butyl acetate into the stirring tank one by one, and stir at 600 r / min until they are evenly mixed to prepare the top coating.
[0124] Example 5
[0125] This example provides a double-layer coating, including a bottom coating and a top coating.
[0126] Among them, the bottom coating, by mass percentage, is composed of: 2% polycarbosilane, 16% titanium precursor, 10% polysiloxane resin, 10% epoxy resin, 10% silicon carbide, 4% basalt flakes, 4% zinc phosphate, 5% low-melting glass powder, 10% copper chromite black, 10% p-xylene, 18.4% propylene glycol methyl ether acetate, 0.5% dispersant, and 0.1% wetting and leveling agent. Its preparation method is as follows:
[0127] (1) Preparation of Component A:
[0128] Weigh 2% polycarbosilane and 16% titanium precursor, and mix them evenly.
[0129] (2) Preparation of Component B:
[0130] Add 10% polysiloxane resin, 10% epoxy resin, 10% p-xylene, and 18.4% propylene glycol methyl ether acetate into a stirrer and stir at 800 r / min until evenly dissolved. Then, add 0.5% dispersant, 0.1% wetting and leveling agent, 10% silicon carbide, 4% basalt flakes, 4% zinc phosphate, 5% low-melting glass powder, and 10% copper chromite black one by one, and pre-stir at 1000 r / min until the materials are evenly mixed.
[0131] Use a sand mill to grind the above premix at 2000 r / min until the fineness is ≤15 μm.
[0132] (3) Preparation of the bottom coating:
[0133] Mix the above Component A and Component B, and stir at 700 r / min until evenly mixed to obtain the bottom coating.
[0134] Among them, the top coating, by mass percentage, is composed of: 20% silica sol, 20% epoxy-modified siloxane, 20% polysilazane, 0.5% anti-graffiti additive, and 39.5% butyl acetate. Its preparation method is as follows:
[0135] Add 20% silica sol, 20% epoxy-modified siloxane, 20% polysilazane, 0.5% anti-graffiti additive, and 39.5% butyl acetate into a stirring tank one by one, and stir at 600 r / min until evenly mixed to obtain the top coating.
[0136] Example 6
[0137] This example provides a double-layer coating, including a bottom coating and a top coating.
[0138] Among them, the composition of the bottom coating by mass percentage is as follows: polyborosilazane 4%, titanium precursor 12%, polysiloxane resin 12%, epoxy resin 17%, silicon carbide 3%, talcum powder 3%, basalt flakes 7%, zinc phosphate 4%, aluminum phosphate 4%, low-melting glass powder 5%, copper chromite black 10%, p-xylene 6%, propylene glycol methyl ether acetate 12.4%, dispersant 0.5%, wetting and leveling agent 0.1%. The preparation method is as follows:
[0139] (1) Preparation of component A:
[0140] Weigh 4% polyborosilazane and 12% titanium precursor, and mix them evenly.
[0141] (2) Preparation of component B:
[0142] Add 12% polysiloxane resin, 17% epoxy resin, 6% p-xylene, and 12.4% propylene glycol methyl ether acetate, and stir at 700 r / min until uniformly dissolved. Then, add 0.5% dispersant, 0.1% wetting and leveling agent, 3% silicon carbide, 3% talcum powder, 7% basalt flakes, 4% zinc phosphate, 4% aluminum phosphate, 5% low-melting glass powder, and 10% copper chromite black one by one, and pre-stir at 1000 r / min until the materials are mixed evenly.
[0143] Use a sand mill to grind the above premix at 2000 r / min until the fineness is ≤15 μm.
[0144] (3) Preparation of the bottom coating:
[0145] Mix the above component A and component B, and stir at 600 r / min until uniform to prepare the bottom coating.
[0146] Among them, the composition of the top coating by mass percentage is as follows: silica sol 30%, polyester-modified polysiloxane 15%, polyborosilazane 12%, anti-graffiti additive 5%, butyl acetate 38%. The preparation method is as follows:
[0147] Add 30% silica sol, 15% polyester-modified polysiloxane, 12% polyborosilazane, 5% anti-graffiti additive, and 38% butyl acetate into the stirring tank one by one, and stir at 700 r / min until uniform to prepare the top coating.
[0148] Comparative Example 1
[0149] This comparative example provides a double-layer coating, including a bottom coating and a top coating.
[0150] Among them, the bottom coating is 100% polyborosilazane.
[0151] The composition of the top coating by mass percentage is as follows: silica sol 25%, epoxy-modified polysiloxane 25%, anti-graffiti additive 1%, butyl acetate 49%. The preparation method is as follows:
[0152] Add 25% silica sol, 25% epoxy-modified silicone, 1% anti-graffiti additive, and 49% butyl acetate into the stirring tank one by one, and stir at 1200 r / min until uniform to prepare the topcoat.
[0153] Comparative Example 2
[0154] This comparative example provides a double-layer coating, including a bottom coat and a top coat.
[0155] Among them, the bottom coat is 100% polysilazane.
[0156] The composition of the top coat by mass percentage is: 45% silica sol, 17% epoxy-modified silicone, 16% polysilazane, 2% anti-graffiti additive, and 20% butyl acetate. The preparation method is as follows:
[0157] Add 45% silica sol, 17% epoxy-modified silicone, 16% polysilazane, 2% anti-graffiti additive, and 20% butyl acetate into the stirring tank one by one, and stir at 1500 r / min until uniform to prepare the top coat.
[0158] Comparative Example 3
[0159] This comparative example provides a coating, including a bottom coat and a top coat.
[0160] Among them, the composition of the bottom coat by mass percentage is: 10% polysilazane, 30% epoxy resin, 10% silicon carbide, 15% basalt scales, 2% white carbon black, 13% copper chromite black, 19.5% p-xylene, and 0.5% dispersant. The preparation method is as follows:
[0161] (1) Preparation of Component A:
[0162] Weigh 10% polysilazane ceramic precursor.
[0163] (2) Preparation of Component B:
[0164] Stir 30% epoxy resin and 19.5% p-xylene at 500 r / min until uniformly dissolved, then add 0.5% dispersant, 10% silicon carbide, 15% basalt scales, 2% white carbon black, and 13% copper chromite black one by one, and pre-stir at 800 r / min until the materials are uniformly mixed.
[0165] Use a sand mill to grind the above premix at 2000 r / min until the fineness ≤ 15 μm.
[0166] (3) Preparation of the bottom coat:
[0167] Mix the above Component A and Component B, and stir at 300 r / min until uniform to prepare the bottom coat.
[0168] Among them, the surface coating is composed by mass percentage as follows: silica sol 35%, epoxy-modified silicone 10%, polysilazane 10%, anti-graffiti additive 4%, butyl acetate 41%. The preparation method is as follows:
[0169] Add 35% silica sol, 10% epoxy-modified silicone, 10% polysilazane, 4% anti-graffiti additive, and 41% butyl acetate into the stirring tank one by one, and stir at 500 r / min until uniform to prepare the surface coating.
[0170] Comparative Example 4
[0171] This comparative example provides a double-layer coating, including a bottom coating and a surface coating.
[0172] The preparation method of the bottom coating is referred to Example 2 in CN 109401618 A, specifically as follows:
[0173] Provide preparation raw materials, the preparation raw materials include polysilazane and polysiloxane. Among them, R1 of the polysilazane is aryl, R2 is hydrogen group, R3 is alkylamine group, the mass percentage of the polysilazane in the preparation raw materials is 40%, R4 of the polysiloxane is cycloalkane, R5 is alkylsiloxy group, and the mass percentage of the polysiloxane in the preparation raw materials is 30%;
[0174] Place the polysilazane and polysiloxane in a reactor, mix the polysilazane and polysiloxane at a speed of 800 revolutions per minute, and the polysiloxane and polysilazane undergo a copolymerization reaction to generate a polysiloxane-polysilazane copolymer;
[0175] Provide dibutyl ether, the mass percentage of the dibutyl ether in the preparation raw materials is 30%, and mix the dibutyl ether and the polysiloxane-polysilazane copolymer at a speed of 1000 revolutions per minute to obtain the bottom coating.
[0176] The preparation of the surface coating is the same as that in Example 1.
[0177] Performance test
[0178] Perform a cross-cut test on the coatings obtained from each example and comparative example according to GB / T 9286 to determine the adhesion of the coating to the substrate (heater substrate, stainless steel).
[0179] The coatings obtained from each example and comparative example were respectively applied to the surface of the heater. For the comparability of test results, the heater material (stainless steel) and shape were the same, and the coating thickness was consistent. Simulating the working environment of the heating tube in an electric water heater, a spiked water quality was used (by adding chemical reagents such as calcium chloride, magnesium chloride, sodium bicarbonate, etc. to the water to adjust the hardness value of the water quality to 400 - 500 mg / L and the chloride ion concentration to 200 - 300 mg / L, making the water quality prone to scale formation and having a certain corrosiveness to metals). An electric heating period of a fixed duration (20 min) and a power-off period of a fixed duration (5 min) was used as one heating cycle, and finally the heating temperature was set within a certain range. The heater was subjected to 150 - 250 heating cycles, and the time point with the most scale increase during this period was used as the comparison time point for the scale inhibition rate. At the same time, in this test environment, the corrosion resistance effects of each group of heaters were compared. The corrosion resistance end point was judged by the heater being corroded through and short-circuit tripping (there was a protection mechanism during the test process). The results are shown in Table 1.
[0180] Table 1
[0181] Scale inhibition rate Spiked water corrosion resistance Crosshatch adhesion Example 1 97% 121h Grade 0 Example 2 99% 118h Grade 0 Example 3 94% 109h Grade 0 Example 4 98% 120h Grade 0 Example 5 91% 99h Grade 1 Example 6 88% 72h Grade 0 Comparative Example 1 89% 97h Grade 0 Comparative Example 2 92% 71h Grade 0 Comparative Example 3 94% 68h Grade 2 Comparative Example 4 63% 102h Grade 0 Blank control / 40h /
[0182] Among them, the blank control was that no coating was applied to the surface of the heater. The scale inhibition rate = (the weight of scale on the surface of the blank heater - the weight of scale on the surface of the heater coated with the coating) / the weight of scale on the surface of the blank heater * 100%. In addition, it should be noted that the spiked water corrosion resistance test of the present invention is an accelerated test. Therefore, the spiked water corrosion resistance time in Table 1 does not represent the actual corrosion time of the product, and this value is only used for comparing and explaining the advantages and disadvantages of each group of coatings.
[0183] Figure 1 The scale state of the heater coated with the coating of Example 1 of the present invention. Figure 2 The scale state of the blank control.
[0184] The above results show that the double-layer coating obtained in the examples of the present invention can be firmly combined with the heater substrate and has good scale resistance and corrosion resistance.
[0185] Finally, it should be noted that the above embodiments are only used to illustrate the present invention, rather than to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, those of ordinary skill in the art should understand that various combinations, modifications, or equivalent replacements of the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention, and should all be covered within the scope of the claims of the present invention.
Claims
1. A two-layer coating, characterized in that, it comprises a bottom coating and a top coating, the bottom coating comprises a ceramic precursor and a resin, the ceramic precursor is composed of a polysilane compound and a metal precursor, the polysilane compound is selected from one or more of polycarbosilane, polyborosilazane, and polysilboron carbonitride, and the metal precursor is selected from one or more of a zirconium precursor, an aluminum precursor, and a titanium precursor.
2. The two-layer coating according to claim 1, characterized in that, the mass ratio of the polysilane compound to the metal precursor is 3:1 - 1:
6.
3. The two-layer coating according to claim 1, characterized in that, the resin is a polysiloxane resin and / or an epoxy resin, preferably a mixture of a polysiloxane resin and an epoxy resin with a mass ratio of 20:0 - 8:15; more preferably, the mass ratio of the ceramic precursor to the resin is 99:1 - 10:
90.
4. The two-layer coating according to any one of claims 1 - 3, characterized in that, the bottom coating further comprises one or more of a filler, a solvent, and an auxiliary agent; preferably, the filler is selected from one or more of silicon carbide, talcum powder, glass flakes, basalt flakes, muscovite, zinc phosphate, aluminum phosphate, low-melting glass powder, silica, and inorganic pigments, and the mass of the filler accounts for 0.1 - 50% of the mass of the bottom coating; the solvent is selected from one or more of alkane solvents, ether solvents, ketone solvents, benzene derivative solvents, and ester solvents, and the mass of the solvent accounts for 0.1 - 50% of the mass of the bottom coating; the auxiliary agent is selected from one or more of a dispersant and a wetting and leveling agent, and the mass of the auxiliary agent accounts for 0.1 - 5% of the mass of the bottom coating.
5. The two-layer coating according to any one of claims 1 - 4, characterized in that, the top coating is composed by mass percentage: 10% - 50% of silica sol, 1 - 25% of epoxy-modified siloxane, 0 - 20% of polysilane compound, 0.1 - 5% of anti-graffiti auxiliary agent, and 10 - 70% of solvent; the solvent is preferably butyl acetate.
6. The preparation method of the two-layer coating according to any one of claims 1 - 5, characterized in that, the preparation method of the bottom coating comprises: mixing the polysilane compound and the metal precursor to obtain a ceramic precursor, namely component A; mixing and grinding the raw materials other than the ceramic precursor to obtain component B, with a fineness ≤ 15 μm; finally mixing component A and component B to obtain the bottom coating; and / or, the preparation method of the top coating comprises: mixing silica sol, epoxy-modified siloxane, polysilane compound, anti-graffiti auxiliary agent and solvent, and then obtaining the top coating, preferably using stirring and mixing, and the stirring rate is 100 - 2000 r / min.
7. A two-layer coating, characterized in that, it is formed by the two-layer coating according to any one of claims 1 - 5.
8. An article with a coating, the article comprises a substrate and a coating attached to at least a part of the surface of the substrate, characterized in that, the coating is the two-layer coating according to claim 7.
9. The article according to claim 8, characterized in that, The substrate is a metal substrate, a glass substrate, a ceramic substrate, an enamel substrate, a polymer substrate, or a composite substrate of two or more of the above substrates.
10. The article according to claim 8, wherein, the article is a household appliance, preferably a water heater.
Citation Information
Patent Citations
Coating composition, preparation method of coating composition, coating part, preparation method of coating part, and household appliance
CN109401618A
Cited By
Double-layer coating and preparation method therefor and use thereof
EP4600320A1