Method for comprehensively recovering valuable elements from waste lithium iron phosphate battery material

Through two-step leaching and lithium phosphate precipitation processes, the problems of low purity and unstable quality of iron products in waste lithium iron phosphate batteries are solved, and efficient recycling of iron, phosphorus and lithium elements are achieved. The obtained products have high purity and good quality, and the production of iron slag is avoided.

CN120157187APending Publication Date: 2025-06-17CENT SOUTH UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202510105310.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-23
Publication Date
2025-06-17

AI Technical Summary

Technical Problem

In the prior art, when recycling waste lithium iron phosphate batteries, the crystal structure of the iron product changes, the product purity is low, and the quality is unstable, making it difficult to meet the requirements of re-preparation of lithium iron phosphate, resulting in serious problems in iron phosphate accumulation.

Method used

The two-step leaching and lithium phosphate precipitation process are adopted to separate sodium phosphate products through the alkali leaching process, and the iron oxide products are separated by acid leaching process, and lithium phosphate products are obtained by adjusting the pH value precipitation to achieve efficient recovery of iron, phosphorus and lithium elements.

Benefits of technology

The recycling efficiency of iron, phosphorus and lithium elements is significantly improved. The obtained iron products and lithium phosphate products are of high purity and good quality, avoiding the generation of phosphorus and iron slag, simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120157187A_ABST
    Figure CN120157187A_ABST
Patent Text Reader

Abstract

The invention discloses a method for comprehensively recovering valuable elements from a waste lithium iron phosphate battery material. The method comprises the following steps: carrying out alkali leaching on black powder and / or pole piece materials of the waste lithium iron phosphate batteries, and then carrying out solid-liquid separation to obtain alkali leaching residues and an alkali leaching solution; carrying out acid leaching on the alkaline leaching residues, and then carrying out solid-liquid separation to obtain an iron oxide powder product and an acid leaching solution; the alkali leaching liquid is cooled and crystallized to obtain a sodium phosphate product and crystallization mother liquor, and the crystallization mother liquor can be circularly used for the alkali leaching process; adjusting the pH value of the acid leaching solution, precipitating and separating to obtain a lithium phosphate product and a lithium precipitation mother solution, wherein the lithium precipitation mother solution can be used for preparing a sodium sulfate product. The method can effectively separate iron, phosphorus and lithium products, and is high in recovery rate, simple, short in process, low in cost and suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for recycling waste lithium iron phosphate battery materials, and specifically to a method for comprehensively recycling valuable elements from waste lithium iron phosphate battery materials, belonging to the technical field of recycling and utilization of lithium-ion batteries. Background Art

[0002] Lithium iron phosphate (LiFePO4) batteries have been widely used in the field of electric vehicles due to their excellent safety performance and environmental protection advantages such as non-toxicity. With the booming development of the electric vehicle market, the consumption of LiFePO4 batteries continues to increase, and a large number of LiFePO4 batteries are retired from electric vehicles every year. Even after the cascade utilization of waste LiFePO4 batteries, the only final option is to be scrapped and recycled. If these waste batteries are not properly treated, it will cause waste of resources and serious environmental pollution problems.

[0003] The developed methods for recycling LiFePO4 batteries include hydrometallurgy and direct regeneration. Hydrometallurgy uses different leaching solutions and precipitants to separately recover valuable metals. The technology is relatively mature, the process flow and equipment are relatively standardized, which is convenient for large-scale production. Currently, there are many industrial application cases and experience accumulations. The direct regeneration method mainly focuses on restoring the electrochemical performance of the battery cathode material, and has limited ability to recover other metal elements. Although the direct regeneration process flow is simple, its regeneration effect is greatly affected by the damage degree of waste batteries, and it has high requirements for the purity of the regenerated material. In large-scale applications, the economic benefits of direct regeneration are not as stable as those of hydrometallurgy. To sum up, hydrometallurgy is more favored in the recycling of lithium-ion batteries. And currently, traditional wet recycling is mainly divided into three categories: acidic total component leaching, acidic oxidation selective leaching, and non-acid oxidation selective leaching. After waste LiFePO4 is leached by a leaching agent, elements such as lithium and iron enter the solution and the leaching residue respectively. After impurity removal, purification, and separation, lithium products and iron products are obtained. Lithium is usually recovered in the form of lithium carbonate and lithium phosphate, and the iron product is mostly iron phosphate. However, when these processes recover iron as iron phosphate, they face problems such as crystal structure change, low product purity, and unstable quality, which are difficult to meet the requirements for re-preparing lithium iron phosphate. These problems make the problem of iron phosphate accumulation more and more serious. Therefore, it is urgent to find other methods that can comprehensively recycle waste lithium iron phosphate cathode materials. Summary of the Invention

[0004] Aiming at the problems existing in the prior art, the purpose of the present invention is to provide a method for comprehensively recycling valuable elements from waste lithium iron phosphate battery materials. This method can significantly improve the recovery efficiency of iron, phosphorus, and lithium elements, and the obtained iron products and lithium phosphate products have high purity and good quality. The method is simple and has low cost.

[0005] In order to achieve the above technical objectives, the present invention provides a method for comprehensively recovering valuable elements from waste lithium iron phosphate battery materials. The method comprises subjecting waste lithium iron phosphate battery black powder and / or electrode sheet materials to alkali leaching and then performing solid-liquid separation to obtain alkali leaching residues and alkali leaching solutions; subjecting the alkali leaching residues to acid leaching and then performing solid-liquid separation to obtain iron oxide products and acid leaching solutions; obtaining sodium phosphate products and crystallization mother liquor I by cooling crystallization of the alkali leaching solutions, and the crystallization mother liquor I can be recycled for the alkali leaching process; and obtaining lithium phosphate products and lithium precipitation mother liquor by adjusting the pH value of the acid leaching solutions for precipitation separation.

[0006] The present invention first separates sodium phosphate products through the alkali leaching process, and then separates iron oxide products (acid leaching residues) from the alkali leaching residues through the acid leaching process. The acid leaching solutions are separated to obtain lithium phosphate products by regulating the pH value, gradually realizing the efficient recovery of iron, phosphorus, and lithium elements. Among them, the iron oxide products have good quality and stable crystal forms, and the lithium phosphate products meet the secondary requirements of the lithium phosphate industry standard for color fluorescent powder. At the same time, the generation of phosphorus-iron slag is avoided.

[0007] As a preferred solution, the lithium precipitation mother liquor is adjusted in pH value and then subjected to extraction separation with an HBL-121 extractant to obtain a lithium-containing organic phase and a raffinate. The lithium-containing organic phase is subjected to back-extraction with hydrochloric acid to obtain a lithium-containing back-extraction solution; the raffinate is subjected to evaporation concentration and cooling crystallization to obtain sodium sulfate products and crystallization mother liquor II; among them, both the lithium-containing back-extraction solution and the crystallization mother liquor II can be recycled for the lithium precipitation process.

[0008] As a preferred solution, the volume ratio of the HBL-121 extractant to the lithium precipitation mother liquor is 1-4:4-1.

[0009] As a preferred solution, the volume ratio of the lithium-containing organic phase to hydrochloric acid is 3-6:1.

[0010] As a preferred solution, the concentration of the hydrochloric acid is 3-6 mol / L.

[0011] As a preferred solution, the evaporation concentration temperature of the raffinate is 100 °C; the cooling crystallization temperature is room temperature.

[0012] As a preferred solution, the particle sizes of the waste lithium iron phosphate battery black powder and the electrode sheet materials are both -100 mesh.

[0013] As a preferred solution, the conditions for the alkali leaching are as follows: the leaching agent is a sodium hydroxide solution; the concentration of the leaching agent is 1-12 mol / L, further preferably 1-6 mol / L, and most preferably 4-6 mol / L; the liquid-solid ratio is 4-10 ml / g, further preferably 5-8 ml / g; the leaching temperature is 40-90 °C, further preferably 45-85 °C, the leaching time is 1-3 h; the pH value of the leaching system is 10-14.

[0014] During the alkali leaching process of the present invention, since NaOH itself has weak oxidizing properties and the oxidation potential of lithium iron phosphate under alkaline conditions is relatively low, it can be directly oxidized to Fe2O3 by NaOH and oxygen in the air. The involved reaction formula is as follows: 12LiFePO4 + 24NaOH + 3O2 → 4Li3PO4↓ + 8Na3PO4 + 6Fe2O3↓ + 12H2O.

[0015] As a preferred embodiment, the cooling crystallization conditions of the alkali leaching solution are: the temperature is -10 to 20°C, and the time is 2 to 48 hours.

[0016] As a preferred embodiment, after adding sodium hydroxide solution to the crystallization mother liquor, it is returned to the alkali leaching process.

[0017] As a preferred embodiment, the alkali leaching residue is washed with water at a temperature not lower than 60°C. After washing the alkali leaching residue, it is dried at 60 to 100°C.

[0018] As a preferred embodiment, the conditions for acid leaching are: the leaching agent is sulfuric acid; the concentration of the leaching agent is 0.1 to 0.8 mol / L; the liquid-solid ratio is 5 to 9 ml / g, and further preferably 6 to 8 ml / g; the leaching temperature is 55 to 85°C, the leaching time is 0.5 to 4 hours; the pH value of the leaching system is 4 to 6.

[0019] As a preferred embodiment, the acid leaching residue obtained after acid leaching is washed and dried to obtain an iron oxide powder product.

[0020] As a preferred embodiment, the drying temperature of the acid leaching residue is not lower than 530°C, and the drying time is 2 to 12 hours.

[0021] As a preferred embodiment, the pH value of the acid leaching solution is adjusted to the range of 8 to 14.

[0022] As a preferred embodiment, the pH value of the lithium precipitation mother liquor is adjusted to the range of 8 to 13.

[0023] As a preferred embodiment, the pH regulator includes alkaline substances such as sodium hydroxide, sodium carbonate, calcium oxide, or calcium carbonate.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The present invention adopts a two-step leaching and lithium phosphate precipitation process. Iron, phosphorus, and lithium in the cathode material are respectively recovered in the forms of iron oxide, sodium phosphate, and lithium phosphate, with a high comprehensive recovery efficiency. Among them, the lithium phosphate product meets the second-level requirements of the lithium phosphate industry standard for color fluorescent powder, and the iron oxide product has high purity, good quality, and stable crystal form; (2)The three products prepared by the present invention have wide applications, and at the same time, the generation of phosphorus-iron slag is avoided, which has very important practical significance in the field of recycling of waste batteries. Compared with the traditional process, it has a broad prospect of industrialization, low cost, and short process. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic process flow diagram of Example 1 of the present invention.

[0026] Figure 2 It is an XRD pattern of the alkali leaching residue in Example 1 of the present invention.

[0027] Figure 3 It is a potential-pH diagram of Fe-Li-P at 65 °C during the alkali leaching process in Example 1 of the present invention.

[0028] Figure 4 It is an XRD pattern of the sodium phosphate product in Example 1 of the present invention.

[0029] Figure 5 It is an XRD pattern of the iron oxide product (acid leaching residue) in Example 1 of the present invention.

[0030] Figure 6 It is an XRD pattern of the lithium phosphate product in Example 1 of the present invention. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0031] In order to make the objectives, technical solutions and advantages of the present invention clearer and more understandable, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0032] Example 1 (1)The black powder of waste lithium iron phosphate batteries is ground to less than 100 meshes.

[0033] (2)The black powder obtained in step (1) is mixed with a 4 mol / L sodium hydroxide solution at a liquid-solid ratio of 7 g / mL, stirred and reacted at 65 °C for 3 h, and then filtered to obtain an alkali leaching residue and an alkali leaching filtrate. Among them, the main components of the alkali leaching residue are iron oxide and lithium phosphate, and their composition is shown in the appendix Figure 2 .

[0034] Figure 3 It is a potential-pH diagram of Fe-Li-P at 65 °C, which reflects the thermodynamic feasibility of the NaOH oxidative leaching method. This diagram shows that the oxidation potential of lithium iron phosphate under alkaline conditions is relatively low and can be directly oxidized to Fe2O3 by NaOH and oxygen in the air.

[0035] (3) Cool the filtrate from the soda ash leaching in step (2) to 10 °C for crystallization for 48 h, filter to obtain filtrate 1 and crystalline product 1, and dry the crystalline product 1 at 40 °C for 24 h to obtain the by-product of sodium phosphate dodecahydrate crystals ( Figure 4 ); After supplementing 3.9 mol / L sodium hydroxide to filtrate 1, it is returned to step (2) as the leaching agent.

[0036] (4) Wash the soda ash leaching residue in step (2) with water at 65 °C (the amount of water used is 3 ml / g), and then mix it with 0.4 mol / L sulfuric acid solution according to a liquid-solid ratio of 8 g / mL. Keep stirring and reacting at 55 °C for 1 h and then filter to obtain the acid leaching residue and acid leaching filtrate. Wash the acid leaching residue with pure water and dry it at 90 °C for 12 h to obtain the by-product of acid leaching residue, and this acid leaching residue is iron oxide powder, and its composition is shown in the appendix Figure 5 .

[0037] (5) Stir and add 10 mol / L sodium hydroxide solution to the acid leaching filtrate in step (4) at 90 °C, adjust the pH to 8.5, carry out precipitation reaction and aging, filter to obtain filtrate 2 and product 2. Wash product 2 with hot water at least 3 times and then dry it at 90 °C for 12 h to obtain the lithium phosphate product, and its composition is shown in the appendix Figure 6 .

[0038] (6) Adjust the pH of the above filtrate 2 (lithium precipitation mother liquor) to 13 with sodium hydroxide, use HBL-121 extractant, with a phase ratio (O-A ratio) of 1:1, shake at room temperature for 10 min to obtain the lithium-containing organic phase and the raffinate. Among them, the lithium-containing organic phase is further subjected to single-stage back-extraction, and the back-extraction agent is 3 mol / L hydrochloric acid solution, with a phase ratio (O-A ratio) of 6:1, shake at room temperature for 10 min to obtain the lithium-containing back-extracted solution, and recycle this lithium-containing back-extracted solution to the lithium precipitation process in step (5).

[0039] (7) Evaporate and concentrate the raffinate obtained in step (6) at 100 °C and then cool it to crystallize at room temperature to obtain the sodium sulfate product, and recycle the crystallization mother liquor to the lithium precipitation process in step (5).

[0040] Through test analysis, in the black powder material of this example, the total recovery rate of phosphorus reaches 92.21%, the total recovery rate of lithium is 98.36%, and the recovery rate of iron is 99.98%.

[0041] Example 2 (1) Grind the waste lithium iron phosphate battery cathode sheet material to less than 100 mesh.

[0042] (2) Mix the cathode sheet material obtained in step (1) with 3 mol / L sodium hydroxide solution according to a liquid-solid ratio of 6 g / mL, stir and react at 45 °C for 2 h and then filter to obtain the soda ash leaching residue and the soda ash leaching filtrate. Among them, the main components in the soda ash leaching residue are iron oxide, lithium phosphate and water.

[0043] (3) Cool the filtrate from the soda ash leaching in step (2) to 10 °C for crystallization for 48 h, filter to obtain filtrate 1 and crystallization product 1. The crystallization product 1 is dried at 40 °C for 24 h to obtain the by-product of sodium phosphate dodecahydrate crystals; after adding 2.9 mol / L sodium hydroxide to filtrate 1, it is returned to step (2) as the leaching agent.

[0044] (4) Wash the soda ash leaching residue in step (2) with water at 45 °C (the amount of water used is 3 ml / g), and then mix it with 0.3 mol / L sulfuric acid solution according to a liquid-solid ratio of 7 g / mL. Stir and react at 55 °C for 1 h and then filter to obtain the acid leaching residue and acid leaching filtrate. The acid leaching residue is washed with pure water and dried at 90 °C for 12 h to obtain the by-product of acid leaching residue, and this acid leaching residue is iron oxide powder.

[0045] (5) Stir and add 10 mol / L sodium hydroxide solution to the acid leaching filtrate in step (4) at 90 °C, adjust the pH to 8.5, carry out precipitation reaction and aging, filter to obtain filtrate 2 and product 2. Product 2 is washed with hot water at least 3 times and then dried at 90 °C for 12 h to obtain the lithium phosphate product.

[0046] (6) Adjust the pH of the above filtrate 2 (lithium precipitation mother liquor) to 13 with sodium hydroxide, use HBL-121 extractant, with a phase ratio (O-A ratio) of 2:1, shake at room temperature for 10 min to obtain the lithium-containing organic phase and the raffinate. Among them, the lithium-containing organic phase is further subjected to single-stage back-extraction, and the back-extraction agent is 6 mol / L hydrochloric acid solution, with a phase ratio (O-A ratio) of 3:1, shake at room temperature for 10 min to obtain the lithium-containing back-extraction solution, and this lithium-containing back-extraction solution is recycled to the lithium precipitation process in step (5).

[0047] (7) The raffinate obtained in step (6) is evaporated and concentrated at 100 °C and then cooled and crystallized at room temperature to obtain the sodium sulfate product, and the crystallization mother liquor is recycled to the lithium precipitation process in step (5).

[0048] Through test analysis, in the positive electrode material of this example, the total phosphorus recovery rate reaches 90.86%, the total lithium recovery rate is 96.2%, and the iron recovery rate is 97.13%.

[0049] Example 3 (1) Grind the black powder of waste lithium iron phosphate battery to less than 100 mesh.

[0050] (2) Mix the black powder obtained in step (1) with 2 mol / L sodium hydroxide solution according to a liquid-solid ratio of 5 g / mL, stir and react at 65 °C for 3 h and then filter to obtain the soda ash leaching residue and soda ash leaching filtrate. Among them, the main components in the soda ash leaching residue are iron oxide, lithium phosphate and water.

[0051] (3) Cool the filtrate from the soda ash leaching in step (2) to 10 °C for crystallization for 48 h, filter to obtain filtrate 1 and crystallization product 1, and dry the crystallization product 1 at 40 °C for 24 h to obtain the by-product of sodium phosphate dodecahydrate crystals; after adding 1.9 mol / L sodium hydroxide to filtrate 1, return it to step (2) as the leaching agent.

[0052] (4) Wash the soda ash leaching residue in step (2) with water at 65 °C (the amount of water used is 3 ml / g), and then mix it with 0.2 mol / L sulfuric acid solution according to a liquid-solid ratio of 6 g / mL, keep stirring and reacting at 55 °C for 1 h, then filter to obtain the acid leaching residue and acid leaching filtrate. Wash the acid leaching residue with pure water and dry it at 90 °C for 12 h to obtain the by-product of acid leaching residue, and this acid leaching residue is iron oxide powder.

[0053] (5) Stir and add 10 mol / L sodium hydroxide solution to the acid leaching filtrate in step (4) at 90 °C, adjust the pH to 8.5, carry out precipitation reaction and aging, filter to obtain filtrate 2 and product 2. Wash product 2 with hot water at least 3 times and dry it at 90 °C for 12 h to obtain lithium phosphate product.

[0054] (6) Adjust the pH of the above-mentioned filtrate 2 (lithium precipitation mother liquor) to 13 with sodium hydroxide, use HBL-121 extractant, with a phase ratio (O-A ratio) of 1:2, shake at room temperature for 10 min to obtain the lithium-containing organic phase and the raffinate. Among them, the lithium-containing organic phase is further subjected to single-stage back-extraction, and the back-extraction agent is 3 mol / L hydrochloric acid solution, with a phase ratio (O-A ratio) of 6:1, shake at room temperature for 10 min to obtain the lithium-containing back-extraction solution, and circulate this lithium-containing back-extraction solution to the lithium precipitation process in step (5).

[0055] (7) Evaporate and concentrate the raffinate obtained in step (6) at 100 °C and then cool and crystallize at room temperature to obtain sodium sulfate product, and circulate the crystallization mother liquor to the lithium precipitation process in step (5).

[0056] Through test analysis, in the positive electrode material of this example, the total phosphorus recovery rate reaches 93.4%, the total lithium recovery rate is 95.81%, and the iron recovery rate is 97.93%.

[0057] Comparative Example 1 Recover lithium iron phosphate by the method of Example 1, the difference is that: the leaching temperature in step (2) is controlled at 35 °C.

[0058] Through test analysis, in the positive electrode material of this comparative example, the total phosphorus recovery rate reaches 70.36%, the total lithium recovery rate is 81.73%, and the iron recovery rate is 79.99%. This is because the low soda ash leaching temperature causes the activity of lithium iron phosphate to decline, and phosphorus rapidly precipitates in the form of sodium phosphate at low temperature, resulting in a decrease in the leaching rate.

[0059] Comparative Example 2 The method of Example 2 was adopted to recover lithium iron phosphate, with the difference that the concentration of the sulfuric acid solution in step (4) was controlled to be 0.9 mol / L.

[0060] Through test analysis, the total phosphorus recovery rate of the cathode material in this comparative example reached 89.97%, the total lithium recovery rate was 91.31%, and the iron recovery rate was 93.98%. Since the increase in acid concentration led to partial leaching of iron, the iron recovery rate decreased relatively.

[0061] Comparative Example 3 The method of Example 3 was adopted to recover lithium iron phosphate, with the difference that the liquid-solid ratio in steps (2) and (4) was controlled to be 3 ml / g.

[0062] Through test analysis, the total phosphorus recovery rate of the cathode material in this comparative example reached 84.58%, the total lithium recovery rate was 86.72%, and the iron recovery rate was 96.89%. This was because the effective surface area of the solution per unit volume was small at a low liquid-solid ratio, resulting in a relatively decreased leaching efficiency.

[0063] The present invention has been described above through specific embodiments and examples. However, these descriptions are only illustrative and should not be construed as limiting the protection scope of the present invention. Without departing from the spirit and protection scope of the present invention, those skilled in the art can make various improvements, modifications, or equivalent replacements to the technical solutions and their implementation manners of the present invention, and these should all fall within the protection scope of the present invention.

Claims

1. A method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials, characterized in that: The waste lithium iron phosphate battery black powder and / or pole piece material are subjected to alkali leaching and solid-liquid separation to obtain alkali leaching residue and alkali leaching solution; the alkali leaching residue is subjected to acid leaching and solid-liquid separation to obtain an iron oxide product and an acid leaching solution; the alkali leaching solution is cooled and crystallized to obtain a sodium phosphate product and a crystallization mother liquor I, and the crystallization mother liquor I can be recycled in the alkali leaching process; the acid leaching solution is precipitated and separated by adjusting the pH value to obtain a lithium phosphate product and a lithium precipitation mother liquor.

2. The method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1, characterized in that: The lithium precipitation mother liquor is extracted and separated by HBL-121 extractant after adjusting the pH value to obtain a lithium-containing organic phase and a raffinate. The lithium-containing organic phase is stripped by hydrochloric acid to obtain a lithium-containing stripping solution. The raffinate is concentrated by evaporation and crystallized by cooling to obtain a sodium sulfate product and a crystallization mother liquor II. The lithium-containing stripping solution and the crystallization mother liquor II can be recycled for the lithium precipitation process.

3. A method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1 or 2, characterized in that: The particle size of waste lithium iron phosphate battery black powder and electrode sheet materials is -100 mesh.

4. A method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1 or 2, characterized in that: The conditions for the alkaline leaching are: the leaching agent is sodium hydroxide solution; the concentration of the leaching agent is 1-12 mol / L; the liquid-solid ratio is 4-10 ml / g; the leaching temperature is 40-90° C., and the leaching time is 1-3 hours.

5. The method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1, characterized in that: The acid leaching conditions are as follows: the leaching agent is sulfuric acid; the concentration of the leaching agent is 0.1-0.8 mol / L; the liquid-solid ratio is 5-9 ml / g; the leaching temperature is 45-85° C., and the leaching time is 1-8 hours.

6. The method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1, characterized in that: The cooling crystallization conditions of the alkaline leaching solution are: temperature of -10 to 20°C and time of 2 to 48 hours.

7. A method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1 or 6, characterized in that: The crystallization mother liquor I is returned to the alkali leaching process after adding sodium hydroxide solution.

8. The method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 1, characterized in that: The pH value of the acid leaching solution is adjusted to a range of 8 to 14.

9. The method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 2, characterized in that: The pH value of the lithium precipitation mother solution is adjusted to a range of 8 to 13.

10. A method for comprehensive recovery of valuable elements from waste lithium iron phosphate battery materials according to claim 2 or 9, characterized in that: The volume ratio of the HBL-121 extractant to the lithium precipitation mother liquor is 1-4:4-1; The volume ratio of the lithium-containing organic phase to hydrochloric acid is 3-6:1.

Citation Information

Cited By

  • Comprehensive utilization method of waste lithium iron phosphate lithium extraction slag

    CN120589707A

  • Recycling method of positive electrode material of lithium iron phosphate battery

    CN121929671A

  • Method for recycling lithium iron phosphate battery cathode material

    CN121929671B